Comparison of masking materials and AOE processes etching fused silica

Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab

AZ resist mask (Recipe name: SiO2_res) PolySi mask (Recipe name: SiO2_psi) Cr mask (Recipe mane: SiO2_met)
Generel description Using a photoresist mask as etching mask is often convenient, since it takes less process steps to make than hard masks. The draw backs using resist as masking material in the AOE on glass is that glass does not transfer heat well and therefore the He cooling in the AOE does not work well on glass substrates. This makes the photoresist turn very hot during the etch and that might burn the resist. Resist also has low selectivity to glass so deep glass etch is not working well with photoresist as masking material. Using Poly Silicon as masking material in the AOE has the advantage over photoresist in the fact that the mask can stand a higher temperature. Then a recipe with higher etch can be used. It also as a higher selectivity so it is possible to etch deeper.The draw back might be higher line width reduction but this has not been expored yet. This recipe with a Cr mask gives the highest etch rate, but the wafer uniformity is not so good.
Substrate
  • Fused silica 100mm
  • Fused silica 100mm
  • Fused silica 100mm
Mask material/thickness
  • AZ resist
  • 4.2µm
  • PolySi
  • 2µm
  • Cr
  • 300nm

Pattern defined in the ICP metal

Coil Power
  • 1300 W
  • 1300 W
  • 1100W
Platen Power
  • 200 W
  • 500 W
  • 180W
Platen temperature
  • 0oC
  • 60oC
  • 60oC
He flow
  • 174 sccm
  • 300 sccm
  • 0 sccm
C4F8 flow
  • 5 sccm
  • 18 sccm
  • 40 sccm
O2 flow
  • 0 sccm
  • 0 sccm
  • 5 sccm
H2 flow
  • 4 sccm
  • 0 sccm
  • 0 sccm
Pressure
  • 4 mTorr
  • 4 mTorr
  • 6 mTorr
Etch rate in fused silica
  • 193.2±0.4nm/min @5min etch (2013-03-26)(50nm Al on back side)
  • 173.5±0.5nm/min @40min etch (2013-03-13) (100nm Al on back side)
  • 208nm/min @(5+5)min (2013-08-27) (no Al on back side, He pressure 6.8T)

± refers to the variation over the wafer.
Reduced etch rate in long etch might be due to resist gone at the end. The polymer/resist left on the wafer after etch was less than 20nm and it looked burned.

  • 448.6±0.6nm/min @40min etch (2013-3-26)

± refers to the variation over the wafer.

  • 562nm/min±4.1nm/min @20min etch (2013-6-7)
Selectivity to mask
  • ~1:1.6 (2013-03-26)
  • ~1:16 (2013-03-26)
  • ~1:77 (2013-6-7)
Linewidth reduction
  • ~4µm for this 17.8µm deep etch
  • ~0.22µm/1µm etch depth
  • ~3µm for this 11.6µm deep etch
  • ~0.26µm/1µm etch depth
Substrate size tried
  • 100 mm wafer
  • 100 mm wafer
  • 100 mm wafer
Images


User results

Done by Joachim Thomsen (student at Nanotech) October 2013

The process flow was:

  • Fused silica wafers
  • Deposition of poly-Si on the wafers: LPCVD poly-Si furnace, recipe poly620, 1h30m: aprox. thickness 700nm
  • Adding AZ resist mask
  • Etching the poly-Si mask: AOE recipe "si_etch": 30s
  • Etching the fused silica: using AOE recipe "m_polysi": 11min10sec

Results: