Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/StandardRecipes

From LabAdviser
Revision as of 10:28, 4 September 2025 by Jmli (talk | contribs)
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)

Feedback to this page: click here

Overview of the standard processes: Processes A, B, C, D and SOI

Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab

The instrument was accepted on the basis of the performance of 5 processes. Below is a general comparison - to find more detailed information, go the web page for each process

Standard processes on the DRIE-Pegasus
Process name Type Purpose Conditions during original runs Best usage
Feature Mask material Etch load Comments
Process A Bosch Fast etch 80 µm trench Photo resist 12-13 % on 6" wafer
Process B Bosch Fast etch 30 µm diameter via Photo resist 12-13 % on 6" wafer
Process C Continuous Very slow etch 50 nm posts Aluminum 99.9 % on 4" wafer
Process D Bosch Smooth sidewall etch 10 µm trench Photo resist 50 % on 6" wafer