This page is written by Evgeniy Shkondin @DTU Nanolab if nothing else is stated.
All images and photos on this page belongs to DTU Nanolab.
The fabrication and characterization described below were conducted in 2021 by Evgeniy Shkondin, DTU Nanolab.


Deposition of ZnO is a standard, well-explored ALD process. Previously (before 2018), DEZ had its independent inlet (A1), which shared the same N2 line with the TiCl4 precursor (A2). The DEZ precursor bottle was placed in a cabinet behind the instrument in the service area, and a long pipe led the precursor to the ALD chamber. This option has been abandoned due to safety reasons. This line was very difficult to purge in case of service. The results that were obtained with the old hardware configuration now remain obsolete. Nowadays, if a user wants to deposit ZnO in ALD-1, diethyl zinc (DEZ) must be mounted in the A-line. If TiCl4 is currently present, it has to be exchanged with DEZ. This is a time-consuming task that requires advanced preparation and ordering.

ZnO ALD deposition using DEZ and H2O

ZnO can be deposited in the range between 100 oC to 225 oC. It is not recommended to increase the temperature above 225oC, as the uniformity suffers due to the precursor decomposition. The maximum temperature can be 250o C. Here, however, the film crystal quality, crystallinity, roughness, etc., differ sufficiently from those prepared at a lower temperature range.

ZnO recipes

Recipe: ZnO

Maximum deposition thickness: 100 nm

Temperature: 100 oC - 250 oC

DEZ* H2O
Nitrogen flow 150 sccm 200 sccm
Pulse time 0.1 s 0.1 s
Purge time 5.0 s 5.0 s

This is a standard recipe of ZnO. It is suitable for coating the flat samples and structures with an aspect ratio of around up to 1:10.

Recipe: ZnOT

Maximum deposition thickness: 100 nm

Temperature: 100 oC - 250 oC

DEZ* DEZ H2O H2O
Nitrogen flow 150 sccm 150 sccm 200 sccm 200 sccm
Pulse time 0.1 s 0.1 s 0.1 s 0.1 s
Purge time 0.5 s 20.0 s 0.5 s 20.0 s


This is a more complicated recipe that allows coating the sample with very high aspect ratio profiles. One SEM example is shown on one of the images below. The recipe is good for deposition on very high aspect ratio structures (with aspect ratio more than 1:20) such as deep trenches, pillars, pores etc. ZnOT recipe can also be used for deposition on polymers at low temperatures (80-120 oC).


DEZ is diethylzinc Zn(CH2CH3)2 or ZnEt2

Deposition characteristics

The deposition rate for ZnO depends on the temperature, see the ALD-window graph below. The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.

Deposition rate

In the graphs below the ZnO thickness vs. number of cycles for deposition temperatures between 100 oC and 250 oC presented. Results have been obtained for <100> 100 mm Si wafers with native oxide, based on ellipsometry study. The optical model used in fitting is based on Tauc-Lorentz and two Lorentz oscillators.


Uniformity across 100 mm wafer

Recipe "ZnO" Samples: 100mm ssp-Si

Results have been obtained for <100> 100 mm Si wafers with native oxide, based on ellipsometry study.

Temperature (°C) / Number of cycles Deposition rate (nm/s) Average thickness (nm) Standard deviation Uniformity (%)
100°C / 500cycles 0.1483 75.67 1.49 3.26
150°C / 500cycles 0.1954 95.32 1.32 2.44
200°C / 500cycles 0.1842 87.97 0.31 0.63
225°C / 500cycles 0.1622 81.09 0.45 1.07
250°C / 500cycles 0.1326 67.92 1.71 3.82




Optical functions

Results have been obtained for <100> 100 mm Si wafers with native oxide, based on ellipsometry study.

SEM images

Images obtained using SEM inspection.

ZnO XPS investigation for elemental trace analysis

Chemical composition of ZnO has been analyzed by XPS method. ZnO samples reveals chemically high quality films with no observable contaminations in temperature range 100 - 250 oC.