Specific Process Knowledge/Thin film deposition/Deposition of Tantalum/Sputtering of Ta
Feedback to this page: click here
All images and photos on this page belongs to DTU Nanolab.
Sputtering of Tantalum
Ta can be DC sputtered in the Sputter-System (Lesker) as well as in the cluster sputter system. You will find information on the pressure, max power, and expected deposition rate for the Sputter-System Lesker (commonly called the "old" Lesker)here in LabAdviser. To see all the deposition parameters used in that machine by others, search the Sputter-System Lesker Process Log in LabManager. Ta has also been deposited in the newer cluster sputter system in the chamber called PC 3 from room temperature to 500 °C. You can search the PC 3 Process Log for further information on deposition parameters.
Below you will find information on the surface roughness of sputtered Ta films from the old Sputter-System (Lesker).
Surface roughness optimization
By Bjarke Thomas Dalslet @Nanotech.dtu.dk
The Lesker CMS 18 sputter system enables the deposition of thin films with varying surface roughness. This roughness was verified to be dependent on the sputtered material, sputter mode (DC or RF), and the substrate bias strength. Other probable factors include sputter power and pressure. Here you find the results for Ta. Similar studies were carried out for SiO2 and Si.
The "Ta" study was done on clean Si substrates. The sputter pressure was 3 mTorr using DC sputtering of a Ta target. Some O2 was added to wafer 25 and 26 to make TaO. To obtain fully oxidized films, up to 30-45% O2 should be added. Consult the thesis of Carsten Christensen for details on TaO.
Ta
| Wafer nr | RF bias (W) | Reactive O2 (%) | Power(W) | Rq (RMS) (nm) | Thickness (nm) |
| blank1 | 0 | 0 | 180 | 0.209 | |
| 16 | 10 | 0 | 180 | 0.36 | 56 |
| 24 | 20 | 0 | 180 | 0.357 | |
| 25 | 20 | 9 | 180 | 0.202 | 110 |
| 26 | 20 | 5 | 180 | 0.194 | 95 |
| 27 | 15 | 0 | 180 | 0.413 | |
| 28 | 25 | 0 | 180 | 0.164 | |
| 31 | 30 | 0 | 180 | 0.3 |