Silicon Nitride Recipe
| Parameter | Recipe name: Slow Etch | Recipe name: Slow Etch2 |
|---|---|---|
| Coil Power [W] | 350 | 200 |
| Platen Power [W] | 25 | 50 |
| Platen temperature [oC] | 20 | 20 |
| H2 flow [sccm] | 15 | 15 |
| CF4 flow [sccm] | 30 | 30 |
| Pressure [mTorr] | 3 | 10 |
Etch rate & uniformity
SRN (LPCVD) etch uniformity on 6″ wafer with Slowetch 2 recipe
SRN (LPCVD) etch uniformity on 6″ wafer with Slowetch recipe
Note: The slowetch recipe has faster etch recipe significantly improves etch rate (~30 nm/min) but leads to reduced uniformity (~2.5%) compared to the slower recipes (<1% uniformity). This highlights a trade-off between throughput and etch uniformity in SRN processing.
With DUV mask on ~300 nm SRN layer
Note: The SEM images illustrate the etched SRN profiles across the wafer, progressing from one edge (left) through the center chip (middle) to the opposite edge (right).
*The process was repeated twice, but only one set of data is presented here.