Tantalum deposition
Tantalum can be deposited by e-beam evaporation and sputter deposition. In the chart below you can compare the different deposition equipment.
Sputtering of Tantalum
E-beam evaporation of Tantalum
Tantalum can be deposited by e-beam assisted evaporation in the Temescal tool.
| E-beam evaporation (Temescal and E-beam evaporator (10-pockets)) | Sputter (Lesker) | Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) | |
|---|---|---|---|
| General description | E-beam deposition of Ta
(line-of-sight deposition) |
Sputter deposition of Ta
(not line-of-sight) |
Sputter deposition of Ta
(not line-of-sight) |
| Pre-clean | Ar ion source (E-beam evaporator Temescal only) | none | RF Ar clean |
| Layer thickness | 10Å to 0.2 µm* | 10Å to ? | 10Å to ? |
| Deposition rate | 0.5Å/s to 10Å/s | ~0.3Å/s | at least in the range 1 Å/s to 4 Å/s |
| Batch size |
|
|
|
| Allowed materials |
|
|
|
| Comment | Tantalum deposition heats the chamber*
Heating to 250 °C available in the 10-pocket e-beam evaporator. |
2-inch Ta target. | 3-inch Ta target.
Heating available to 600 °C. |
* The max thickness is limited to 200 nm as Ta deposition heats the chamber. If you wish to deposit more than that, it has to be done in several steps. The temperature on the back of a Si wafer rose to above 160 °C during deposition of 40 nm Ta even when using a cooling plate. If you wish to e-beam deposit Ta, please contact the Thin film group.