Go to 'IBE/IBSD Ionfab 300' equipment page


Acceptance test for SiO2 deposition (2011) on IBE/IBSD Ionfab 300+)

. Acceptance Criteria

Acceptance Result 1

Acceptance Result 2

Substrate information
  • 50 mm SSP Si wafer
  • 525 µm thick
  • Supplied by Nanolab
  • 100 mm SSP Si wafer
  • 525+-25 µm thick
  • 100 mm SSP Si wafer
  • 525+-25 µm thick
Material to be deposited
  • SiO2

The purpose of the SiO2 is to be part of a mirror: <br\> 5 quarter wavelength pairs of <br\> SiO2 <br\> TiO2 <br\> Extra quarter wavelength layer of <br\> TiO2 <br\> 5 quarter wavelength pairs of <br\> SiO2 <br\> TiO2 <br\> Design wavelength (for refractive indices and layer thicknesses): 1300nm <br\> The acceptance criteria is set up for the single SiO2 and TiO2 layers. <br\> Five runs in a row for each material.

  • SiO2
  • SiO2
Deposition thickness
  • 222 nm
  • ~215 nm
  • 224nm
Deposition rate
  • 6 nm/min
  • 7.42 nm/min +- 0.04nm/min

One standard deviation

  • 7.73 nm/min

Only made once

Thickness uniformity
  • <+-1%
  • +-(0.46% +-0.10%)
  • +-0.45%
Reproducibility
  • <+-1.5%
  • +-0.6%
  • Not measured
Stress
  • <500 MPa
  • ~600 MPa
  • 475 MPa
Refractive index .
  • 1.490+-0.004 (stddev wafer to wafer)
  • 1.482+-0.002 (stddev on wafer)


Recipe 1 Recipe 2
Platen angle 15 degrees 10 degrees
Platen rotation speed 20 rpm 20 rpm
Ar(N) flow 4 sccm 4 sccm
Ar(dep. source) flow 9 sccm 8 sccm
I(N) 310 mA 320 mA
Power 675 W 700 W
I(B) 310 mA 280 mA
V(B) 1200 V 1100 V
Vacc(B) 400 V 400 V
Deposition time 29 min 37 min


Other results

Roughness of the surface

Measured with the Optical profiler - PSI mode (on one sample from the acceptance test): Sa= 0.6 nm

Uniformity and break down voltage by Mathias Engholm 2016-11-29

Mathias made 105.62nm SiO2 on a test silicon wafer and on his sample wafer. The sample wafer had gold/Cr on the surface and that had to be electrically isolated. The uniformity over the wafer of the oxide was 0.19% over 9 points - this is better than he has achieved when oxidizing in a furnace. He anodic bonded the wafer without problems. He measured the breakdown voltage and got 0.82+/+ 0.13 V/nm over 24 points. This is just as good as the oxide from the furnaces. Before his deposition he ran a 20 min heat up and 40min dummy deposition to clean the target. This was done with a bright new target and with the small deposition grids mounted.

 
Breakdown voltage over the wafer, by Mathias Engholm 2016-11-29
 
Thickness uniformity over the wafer, by Mathias Engholm 2016-11-29