Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142-pxnano2

From LabAdviser

nano1.42 versus pxnano2

Recipe nano1.42 pxnano2
Tool align="center" Pegasus ASE
Parameters Gas C4F8 75 sccm, SF6 38 sccm D: C4F8 50 sccm E: C4F8 50 sccm, SF6 50 sccm
Power 800 W CP, 40 W PP D: 500 W CP E: 350 W CP, 30 W PP
Pressure 4 mTorr, Strike 3 secs @ 15 mTorr 10 mTorr
Temperature -20 degs 20 degrees
Hardware 100 mm Spacers ?
Time 120 secs D: 3 secs, E: 5 secs, total 12 cycles or 96 secs
Conditions Run ID 2150 wf_2e09b_mar23
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs none
Mask 211 nm zep etched down to 80 nm 211 nm zep etched down to 130 nm