Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142-pxnano2
nano1.42 versus pxnano2
gf | nano1.42 | pxnano2 | |
---|---|---|---|
Tool | Pegasus | ASE | |
Recipe | Gas | C4F8 75 sccm, SF6 38 sccm | |
Pressure | 4 mTorr, Strike 3 secs @ 15 mTorr | ||
Power | 800 W CP, 40 W PP | ||
Temperature | -20 degs | ||
Hardware | 100 mm Spacers | ||
Time | 120 secs | ||
Conditions | Run ID | 2017 | |
Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | ||
Mask | 211 nm zep etched down to 82 nm |
- The results
-
The 30 nm trenches etched 120 seconds nano1.42
-
The 30 nm trenches etched 96 seconds pxnano2
-
The 60 nm trenches etched 120 seconds
-
The 60 nm trenches etched 96 seconds
-
The 90 nm trenches etched 120 seconds
-
The 90 nm trenches etched 96 seconds
-
The 120 nm trenches etched 120 seconds
-
The 120 nm trenches etched 96 seconds
-
The 150 nm trenches etched 120 seconds
-
The 150 nm trenches etched 96 seconds