The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here


Important: The recipes and results listed on this page have been made in 2017. Updated results and recipes from 2019 can be found here.

The ALD temperature window for HfO2 is 150 - 300 oC.

The TEMAHf precursor is heated to 125 oC (TE210) and the heater (TE211 max.) is set to 140 oC during deposition. Remember to set the values in the "MANUAL" tab and to change them to back after deposition (TE211 max. to 1 oC). These values may not be exceeded to prevent precursor decomposition. Due to the heating of the precursor the stabilization time needs to be set to 60 min. Else an alarm (TE210 PID limit exceeded while pulsing) will be triggered and the process will be stopped after the first pulsing attempt.


HfO2 standard recipe

HfO2 deposition using TEMAHf and H2O precursors

The following tables show the recipe and boost settings for the TEMAHf precursor:

TEMAHf H2O
Nitrogen flow 150 sccm 120 sccm
Pulse time 1.6 s 0.1 s
Purge time 8.0 s 4.0 s


Boost flow 500 sccm
Pre-empty 0.5 s
Master fill 1.2 s
Post-empty 0 s


HfO2 deposition at 150 oC

Two HfO2 depositions were made January 2018 - One for 91 cycles and one for 250 cycles. Both deposition were done on 4" wafers with native oxide. The deposition temperature was 150 oC , and the precursor temperature (T210) for TEMAHf was 125 oC.


Number of cycles: 91

Results:

Average HfO2 thickness: 9.57 nm (measured in nine points)
Deposition rate: 0.11 nm/cycle
Non-uniformity: 4.15 %

Number of cycles: 250

Results:

Average HfO2 thickness: 27.65 nm (measured in five points)
Deposition rate: 0.11 nm/cycle
Non-uniformity: 2,20 %

HfO2 deposition at 250 oC

The test was done with 300 cycles at 250 oC where the deposition rate was measured to be 0.0827 nm/cycle. The precursor temperature (T210) for TEMAHf was 125 oC.


Parameter Average Min. Max. Std.Dev %Range
Thickness (nm) 24.83 24.05 27.13 0.68 12.38


The XPS measurement was made by our XPS K-Alpha and shows that the film is purely HfO2 except for some impurities on the surface.


Tanja Amport, Pernille Voss Larsen and Mikkel Dysseholm Mar, DTU Nanolab (former DTU Danchip), 2017.