GaN etching using III-V ICP

Recipe GaN Etch GaN Etch for Si check
Cl2 flow 30 sccm 27 sccm
Ar flow 10 sccm 3 sccm
BCl3 flow 0 sccm 3 sccm
Platen power 200 W 75 W
Coil power 600 W 400 W
Pressure 2 mTorr 4 mTorr
Platen chiller temperature 20 oC 20 oC


Results (GaN Etch)
GaN etch rate 550-580 nm/min
SiO2 etch rate 110-120 nm/min
Sidewall angle ~ 90 o


Results (GaN Etch for Si check)
Si etch rate ~200 nm/min (bghe 2017-01-17) full 4" wafer


 
Result of GaN etching. Oleksii Kopylov, DTU Photonics, 2011.