Jump to content

Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)/Si etch using AOE

From LabAdviser

This page is under construction!!!

Si mask etch has been tried out by Yunhong Ding @ Fotonik


Parameter Si_etch
Coil Power [W] 800
Platen Power [W] 30
Platen temperature [oC] 20
C4F8 flow [sccm] 55
SF6 flow [sccm] 75
Pressure [mTorr] 20


Typical results Resist mask
Si etch rate [nm/min] ~1.12my/min tested by Yunhong Ding @fotonik
Selectivity [:1] ~2.6 tested by Yunhong Ding @fotonik
Profile [o] not tested
Images .
Comments The profile is supposed to be ~88dg but it has not been confirmed