Test data on Cr etch development by Anders Simonsen @NBI.KU 
Final recipe/result for Cr etch and etching down in the nitride in the AOE
DOE experiments and results made on pattern free samples and samples patterned with UV lithography (SEM images)
| Name | Pressure [mTorr] | Coil power [W] | Platen power [W] | Total Flow (Cl2+O2) [sccm] | O2 % | Selectivity | Etch-rate [nm/min] | Side-angle | Corner | Resist-damage | Etch time [s] | Etch depth [nm] | Angle1 | Radius1 | Angle2 | |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| t5 | 5 | 300 | 25 | 40 | 25 | 0.21 | 49.03 | 25.5 | 319.5 | 1 | 175 | 57 | 28 | 331 | 23 | |
| t7 | 15 | 300 | 15 | 40 | 15 | 0.61 | 52.15 | 12 | 154.5 | 1 | 130 | 87 | 14 | 159 | 10 | |
| t8 | 5 | 500 | 15 | 40 | 25 | 0.4 | 49.50 | 39.5 | 228.5 | 1 | 120 | 101 | 42 | 169 | 37 | |
| t4 | 15 | 500 | 25 | 40 | 15 | 0.39 | 70.80 | 19.5 | 201 | 1 | 100 | 82 | 21 | 158 | 18 | |
| t2 | 5 | 300 | 25 | 80 | 15 | 0.21 | 40.54 | 40.5 | 262.5 | 3 | 185 | 75 | 42 | 274 | 39 | |
| t10 | 15 | 300 | 15 | 80 | 25 | 0.68 | 58.00 | 11.5 | 87 | 2 | 120 | 84 | 14 | 70 | 9 | |
| t6 | 5 | 500 | 15 | 80 | 15 | 0.43 | 49.24 | 29.5 | 300 | 5 | 145 | 81 | 29 | 362 | 30 | |
| t9 | 15 | 500 | 25 | 80 | 25 | 0.41 | 80.67 | 18.5 | 134.5 | 2 | 90 | 79 | 20 | 155 | 17 | |
| t1 | 10 | 400 | 20 | 60 | 20 | 0.35 | 63.13 | 17.5 | 288 | 2 | 115 | 79 | 20 | 292 | 15 | |
| t1R | 10 | 400 | 20 | 60 | 20 | 0.4 | 57.14 | 20 | 186 | 2 | 105 | 100 | 24 | 232 | 16 |
Sem images of the DOE
- Sample t5
- Sample t7
- Sample t8
- Sample t4
- Sample t2
- Sample t10
- Sample t9
- Sample t1
- Sample t1R
Tests made after DOE with e-beam patterned samples
| Recipe | Pressure [mTorr] | Coil power [W] | Platen power [W] | Total Flow Cl2+O2 [sccm] | O2% | Temp | Time [s] | CSAR etch rate [nm/min] | CSAR rate w bond | Etch rate [nm/min] | Selectivity | coil load | coil tune | plat load | plat tune | Comment | |||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| test11 | 15 | 300 | 15 | 40 | 25.00 | 20 | 23 | 80.87 | 73 | 52.17 | 0.65 | ||||||||
| test12 | 20 | 300 | 15 | 30 | 23.33 | 20 | 21 | 65.71 | 56 | 57.14 | 0.87 | There seems to been a foot on the Cr after the Cr etch, therefor it was repeated for 2 min Cr etch to remove the foot | |||||||
| test13/laqs | 10 | 300 | 15 | 30 | 23.33 | 20 | 28 | 100.71 | 42.86 | 0.43 | This recipe was chosen over no. 12 because it did not need a large over etch of the Cr (no foot). | ||||||||
| test14 | 10 | 300 | 15 | 40 | 25.00 | 20 | 30 | 88.00 | 40.00 | 0.45 | |||||||||
| nano | 5 | 500 | 15 | 60 | 0.17 | 10 | 33 | 99.00 | 36.36 | 0.37 | 41 | 52 | 31 | 50 | With strike pressure | ||||
| langman | 10 | 500 | 25 | 40 | 0.20 | 8 | 21 | 168.39 | 57.14 | 0.34 | 42 | 52 | 35 | 53 | With strike pressure |
SEM images of the tests after the DOE
These SEM images where done after both the Cr etch and the silicon nitride etch in the ICP metal using the recipe "Slow etch with carrier". The important thing was to see how well the Cr work for masking the nitride given vertical and smooth sidewalls.
- Sample test11
- Sample test12 1 min etch in Cr
- Sample test12 2 min etch in Cr
- Sample test13
- Sample testnano