Measurement of Film Thickness and Optical Constants
Thickness measurement of thin films can be done by optical measurement methods. We have two techniques for this: Ellipsometry (ellipsometer) and Reflectivity measurement (FilmTek+Optical Profiler). If the thin film is not transparent for light then you must find another way to measure the thickness. You can ex. etch a pattern down to the next layer or substrate and then measure the etch step by profilometry. See description further down.
Measurement if the optical constants of a thin film is measured together with the thickness of the film either by ellipsometry (using the ellipsometer),or by refraction (using the FilmTek).
Comparison of the different metodes
| FilmTek 4000 | Ellipsometer | Optical Profiler | Etch/stylus metod | |
|---|---|---|---|---|
| Generel description | Thin films up to 250 µm, Especially good for thick thin films and for wafer mapping | Good for very thin films down to a few Å | Thin films up to 20µm, especially good for measuring in a small point (down to 4µm) | Technique for thickness measurement for non-transparent films |
| Method | Reflection | Ellipsometry | Reflection | Etch combined with stylus profiling |
| Film thickness range | <250 µm (for silicon oxides > ~75nm, thinner layer can be measured using the UV light source) | 20 Å to ~2µm (for silicon oxide) | ~30nm-20µm (down to 10nm when using the base without the microscope) | ~100nm-several micrometers |
| Film thickness accuracy | Very dependent of how good the model fits (if the fit is good it could be within 1% for a single layer) | Very dependent of how good the model fits. | Very dependent of how good the model fits.(Not so good fitting posibility) | Depends on how good the end-stop works |
| Index range | not any limits | not any limits | not any limit | No index measurement |
| Index accuracy | not known | not known | not know | not relevant |
| Wavelength range | 400-1000 nm (with UV source down to 250nm) | 210-1690 nm | 350-950 nm | Not relevant |
| What kind of thin films can be measured | Any film that is transparent to the light in the given wavelength range
ex:
|
Any film that is transparent to the light in the given wavelength range
ex:
|
In principle any film that is transparent to the light in the given wavelength range. It is limited by the refractive index files in the software and only one model (Cauchy)
ex:
|
|
| Substrate size |
|
|
|
Limited by the etching method and the stylus profling instrument. |
| Allowed materials |
|
|
|
|