Descum results

Plasma asher 1

ashing time (min)
1 2 5 7 10 10
Recipe O2 flow N2 flow Power Etched Thickness (nm)
1 70 70 150 14,2 16,3 47,6 123,2 854,3 862,1
2 500 0 200 8,1 32,9 271,1 495,6 446,2