Specific Process Knowledge/Thin film deposition/ALD2 (PEALD)/TiO2 deposition using ALD2
Appearance
Feedback to this page: click here
Result from acceptance test
TiO2 deposition at 150 C (amorphous TiO2) using TiCl4 and H2O precursors
The test was done with 500 cycles where the growth rate was measured to be 0.0385 nm/cycle.
| TiCl4 | H2O | |
|---|---|---|
| Nitrogen flow | 150 sccm | 200 sccm |
| Pulse time | 0.1 s | 0.1 s |
| Purge time | 3.0 s | 4.0 s |
-
Uniformity profile across 150 mm Si wafer based on 13 measurement points measured with ellipsometer. The values for the grown oxide thickness can be seen in the table below.
| Parameter | Average | Min. | Max. | Std.Dev | %Range |
|---|---|---|---|---|---|
| Thickness (nm) | 19.27 | 18.70 | 19.82 | 0.34 | 5.7947 |
-
AFM measurement roughness 0.209 nm.
TiO2 deposition at 300 C (anastase TiO2) using TiCl4 and H2O precursors
The test was done with 500 cycles there the growth rate was measured to be 0.0409 nm/cycle.
| TiCl4 | H2O | |
|---|---|---|
| Nitrogen flow | 150 sccm | 200 sccm |
| Pulse time | 0.1 s | 0.1 s |
| Purge time | 3.0 s | 4.0 s |
-
Uniformity profile across 150 mm Si wafer based on 13 measurement points measured with ellipsometer. The measured oxide thickness is also shown in the table below.
| Parameter | Average | Min. | Max. | Std.Dev | %Range |
|---|---|---|---|---|---|
| Thickness (nm) | 20.46 | 19.85 | 21.02 | 0.35 | 5.6791 |
-
AFM measurement roughness 0.641 nm.
TiO2 on trenches
| TiCl4 | TiCl4 | H2O | H2O | |
|---|---|---|---|---|
| Nitrogen flow | 150 sccm | 150 sccm | 200 sccm | 200 sccm |
| Pulse time | 0.1 s | 0.1 s | 0.1 s | 0.1 s |
Other references
Since the ALD2 is very similar to the ALD1 if the thermal lid is installed you might want to get further information, which can be found here.