Jump to content

Specific Process Knowledge/Etch/Aluminum Oxide/Al2O3 Etch with ICP Metal

From LabAdviser

Feedback to this page: click here


THIS PAGE IS UNDER CONSTRUCTION

Parameter Recipe name: no name yet (testing recipe)
Coil Power [W] 1200
Platen Power [W] 200
Platen temperature [oC] 0
BCl3 flow [sccm] 60
Cl2 flow [sccm] 30
Pressure [mTorr] 4


Etch rates in different materials using the standard "Silicon oxide etch with resist mask"

Material to be etched Etch rate using the above parameters
Al2O3
  • ~230nm/min (1/4 wafer on 6" carrier)