This page describes non standart recipes including multilayers structures.

Low temperature deposition of Al2O3

Recipe: Al2O3 LT

Temperature: 80-150 oC

TMA H2O
Nitrogen flow 150 sccm 200 sccm
Pulse time 0.1 s 0.2 s
Purge time 5.0 s 10.0 s

Deposition rate: 0.089 nm/cycle (@120 oC)



Al2O3 deposition at 100 oC and 150 oC


Deposition conditions at 100 oC
Number of cycles Thickness (nm) Uniformity across 100mm Si substrate (%) Standard deviation error Refractive index @ 632.8 nm
150 14.11 2.18 0.225 1.56
300 25.94 0.68 0.14 1.59
500 41.35 1.87 0.60 1.59
800 65.05 2.28 1.13 1.59
1088 87.25 2.15 1.35 1.60


%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%%

Low temperature deposition of TiO2

Recipe: TiO2 LT

Temperature: 80-150 oC

TiCl4 H2O
Nitrogen flow 150 sccm 200 sccm
Pulse time 0.2 s 0.2 s
Purge time 10.0 s 15.0 s

Deposition rate: 0.048 nm/cycle (@ 120 oC)

Low temperature grown multilayers on flat surfaces

Recipe: EMA01

Recipe: EMA02

Recipe: EMA03

Recipe: EMA04

Temperature: 120 oC

Al2O3/TiO2 multilayers on high aspect ratio structures

Recipe: Multi T

Temperature: 150 oC




Evgeniy Shkondin, DTU Danchip, 2014-2016.