At the moment DANCHIP has 3 PECVDs that can deposite silicon nitride and silicon oxynitride. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.

Recipes on PECVD2 for deposition of silicon nitride and silicon oxynitride

Recipes

Recipe name SiH4 flow [sccm] NH3 flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
SINSTD80 30 20 1000 500 80
SINSTD96 30 20 1000 500 96
1SiN 40 20 1000 700 150

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%] Stress [MPa] BHF etch rate [Å/min] Comments
1SiN

Deposition rate in the middle of two wafers: 49nm/min+-1nm/min (2015-04-24 BGHE)
In the middel: 72.6-76.4 nm/min (2014-08-13 BGHE) Old shower head
Variation over 3 wafers: 71.4-78.6 nm/min (2014-08-13 BGHE) Old shower head

~2-4% (2015-04-24 BGHE)
~5% in the middel (4") (2014-08-13 BGHE) Old shower head
~10% over 3 wafers (2014-08-13 BGHE) Old shower head

SINSTD80 68nm/min (2014-07-07 JML)
SINSTD96


Recipes on PECVD3 for deposition of silicon nitride and silicon oxynitride

Quality Controle (QC) for PECVD3
QC Recipe: QCNITRIDE
SiH4 flow 30 sccm
NH3 flow 30 sccm
N2 flow 1470 sccm
Pressure 650 mTorr
RF-power
  • LF: 30 W 2s
  • HF: 20 W 6s
QC limits PECVD3
Depoition rate 10.4 - 13.0 nm/min
Non-uniformity <2.0 %
Refractive Index 1.909 - 2.028


Recipes

Recipe name SiH4 flow [sccm] NH3 flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
MFSiNLS2 30 30 1470 845 100HF 7.8s

100LF 2.2s

Low stress nitride - standard recipe. The latest measured values can be seen in the process control sheet in LabManager.
MFSiNLS 30 30 1470 650 20HF 6s

30LF 2s

Low stress nitride - old standard recipe. This one is not running well any more.
LFSiN 30 15 1470 550 60LF Compressive stress
HFSiN 30 42 1470 900 20HF Tensile stress

LF=Low Frequency HF=High Frequency MF=Mixed Frequency SiN=Silicon Nitride LS=Low Stress

Expected results

Recipe name Deposition rate [Å/min] RI Uniformity [%]
[Std./mean]
Stress [MPa] KOH etch rate [Å/min] BHF etch rate [Å/min]
MFSiNLS2 ~422 (bghe Feb 2016) ~2.03 ~2 ~6 (bghe Feb 2016) ~2.1 (bghe Feb 2016) ~?
MFSiNLS ~107 ~1.99 ~4 ~-30 ~2.5 ~250
LFSiN ~550 ~1.96 ~3 ~-630 . .
HFSiN ~130 ~1.97 ~2 ~460 . .

Recipes on PECVD1 for deposition of silicon nitride and silicon oxynitride. Expired!:PECVD1 has been decommissioned

Recipes

Recipe name SiH4 flow [sccm] NH3 flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
1nitride 30 20 1000 500 80
1nit_std 40 20 1960 550 60 Process control recipe

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%] Stress [MPa] BHF etch rate [Å/min] Comments
1nitride
1nit_std ~32 1.89 ~1 ~700 The latest measured values can be seen in the process control sheet in LabManager