THIS PAGE IS UNDER CONSTRUCTION

Feedback to this page: click here


The ALD window for depostion of Titanium oxide ranges from 120 oC to 350 oC. XPS measurements shows that at temperatures below 120 oC the TiO3 layer will be contaminated by Cl molecules.

All results shown on this page have been obtained using the "TiO2" recipe on new Si(100) wafers with native oxide:


Recipe: TiO2

Temperature: 150 oC - 350 oC

TMA H2O
Nitrogen flow 150 sccm 200 sccm
Pulse time 0.1 s 0.1 s
Purge time 3.0 s 4.0 s



In the graphs below the Al2O3 thickness as function of number of cycles for deposition temperatures between 150 oC and 350 oC can be seen. From the equations the number of cycles required for a certain thickess can be calculated.






In the graphs below the TiO2 thickness as function of number of cycles for deposition temperatures between 150 oC and 350 oC can be seen. From the equations the number of cycles required for a certain thickess can be calculated.