Deposition of Silver
Silver can be deposited by e-beam evaporation, by sputtering and by thermal evaporation. In the chart below you can compare the different methods on the different deposition equipment.
| E-beam evaporation (Alcatel) | Thermal evaporation (Wordentec) | E-beam evaporation (PVD co-sputter/evaporation) | Sputter evaporation (PVD co-sputter/evaporation) | Sputter evaporation (Wordentec) | |
|---|---|---|---|---|---|
| General description | E-beam deposition of Ag | Thermal deposition of Ag | E-beam deposition of Ag | Sputter deposition of Ag | Sputter deposition of Ag |
| Pre-clean | RF Ar clean | RF Ar clean | RF Ar clean | RF Ar clean | RF Ar clean |
| Layer thickness | 10Å to 1µm* | 10Å to 0.5µm (0.5µm not on all wafers) | 10Å to 1000Å | 10Å to about 5000Å | 10Å to about 3000Å |
| Deposition rate | 2Å/s to 15Å/s | 1Å/s to 10 Å/s | About 1Å/s | Dependent on process parameters. | Depending on process parameters (see logbook) |
| Batch size |
|
|
|
|
|
| Allowed materials |
|
|
|
|
|
| Comment | Only very thin layers. | Only very thin layers (up to 100nm). |
* For thicknesses above 200 nm permission is required.
Thermal deposition of Silver - Process settings for thermal deposition of Silver in Wordentec