Deposition of Silver

Silver can be deposited by e-beam evaporation, by sputtering and by thermal evaporation. In the chart below you can compare the different methods on the different deposition equipment.


E-beam evaporation (Alcatel) Thermal evaporation (Wordentec) E-beam evaporation (PVD co-sputter/evaporation) Sputter evaporation (PVD co-sputter/evaporation) Sputter evaporation (Wordentec)
Batch size E-beam deposition of Ag Thermal deposition of Ag E-beam deposition of Ag Sputter deposition of Ag Sputter deposition of Ag
Pre-clean RF Ar clean RF Ar clean RF Ar clean RF Ar clean RF Ar clean
Layer thickness 10Å to 1µm* 10Å to 0.5µm (0.5µm not on all wafers) 10Å to 1000Å 10Å to about 5000Å 10Å to about 3000Å
Deposition rate 2Å/s to 15Å/s 1Å/s to 10 Å/s About 1Å/s Dependent on process parameters. Depending on process parameters (see logbook)
Batch size
  • Up to 1x4" wafers
  • smaller pieces
  • 6x6" wafers or
  • 6x4" wafers or
  • 24x2" wafers
  • 4x6" wafers or
  • 12x4" wafers or
  • 12x2" wafers
  • 4x6" wafers or
  • 12x4" wafers or
  • 12x2" wafers
  • 6x6" wafers or
  • 6x4" wafers or
  • 24x2" wafers


Allowed materials
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Photoresist
  • PMMA
  • Mylar
  • SU-8
  • Metals
Comment Only very thin layers. Only very thin layers (up to 100nm).

* For thicknesses above 200 nm permission is required.

Thermal deposition of Silver - Process settings for thermal deposition of Silver in Wordentec