Specific Process Knowledge/Etch/Etching of Gold
Appearance
Etching of Gold
Etching of Gold is done wet at Danchip. We have two different solutions:
- KI:I:HO - 400g:100g:400ml?
- HNO:HCl - 1:3
Comparing the two solutions
| Iodine based gold etch | Aqua Regia (Kongevand) | |||||
|---|---|---|---|---|---|---|
| General description |
Etch of pure Gold |
Etch of pure Gold | ||||
| Chemical solution | KJ:J:HO 100g:25g:500ml | H:HO_3 | Process temperature | 20 oC | 20 oC | |
| Possible masking materials: |
Photoresist (1.5 µm AZ5214E) |
Photoresist (1.5 µm AZ5214E) | ||||
| Etch rate |
~100 nm/min (Pure Al) |
~60(??) nm/min | ||||
| Batch size |
1-25 wafers at a time |
1-25 wafer at a time | ||||
| Size of substrate |
4" wafers |
4" wafers | ||||
| Allowed materials |
|
|