Jump to content

Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF)

From LabAdviser

Feedback to this page: click here


Wet Silicon Oxide Etch (BHF and SIO Etch (wetting agent))

Wet Silicon Oxide Etch (BHF): positioned in cleanroom 3
SIO etch (BHF with wetting agent): positioned in cleanroom 4
BHF between the KOH baths: positioned in cleanroom 3. This is primarily used to remove oxide before and after a KOH etch
PP-bath: positioned in fume hood in cleanromm 2


Silicon oxide can be etched using HF. At Danchip it is mainly used in a buffered version BHF (premixed). The BHF has a more stable etch rate and is more gentle to photoresist due to an almost pH neutral solution which makes photoresist a good masking material for the oxide etch.

SIO etch (BHF with wetting agent) can also be used for etching silicon oxide. This is mainly for etching small holes. If you have wetting problems in BHF try the SIO etch. It is also a good idea to wet the sample in water for a few minutes before etching.

Wafers with metals or other materials, not allowed in the dedicated oxide etch baths, can be etched in the PP-bath positioned in the fume hood in cleanroom 2 or in a plastic beaker.

Silicon oxide etch data

BHF 5% HF 40 % HF SIO
General description

Etching of silicon oxide with a stable etch rate

Mainly for removing native oxide

Mainly for etching deep into borofloat or quartz wafers

Etching of silicon oxide - especially for etching small holes

Link to safety APV and KBA see APV here

see KBA here

see APV here

see KBA here

see APV here

see KBA here

see APV here

see KBA here

Chemical solution BHF 5% HF 40% HF BHF with wetting agent
Process temperature Room temperature Room temperature Room temperature Room temperature
Possible masking materials
  • Photoresist
  • Silicon nitride
  • PolySi
  • Blue film

In RCA bench:

  • No masking material

In plastic beaker or PP-bath in the fume hood in cleanroom 2:

  • Photoresist
  • Silicon nitride
  • PolySi
  • Blue film

In RCA bench:

  • No masking material

In plastic beaker with magnetic stirrer in the fume hood in cleanroom 2:

  • Photoresist
  • Silicon nitride (Only on quartz wafers)
  • PolySi(Only on quartz wafers)
  • Blue film
  • Chromium and gold
  • Photoresist
  • Silicon nitride
  • PolySi
  • Blue film
Etch rate
  • Wet thermal oxide:~80nm/min
  • PECVD1 (standard):~147nm/min
  • TEOS:~265nm/min
  • Stoichiometric Si3N4: ~0.75nm/min (Morten Bo Mikkelsen, March 2013)
  • Low stress Si3N4: ~0.38 nm/min (Eric Jensen, Juni 2013)
  • Wet thermal oxide:~25nm/min
  • PECVD1 (standard):~87nm/min
  • TEOS:~153nm/min
  • Boronfloat and quartz: ~3-4 μm/min

A little higher etch rates than BHF

Life time of the photoresist ~½ hour ~½ hour ~½ hour ~½ hour
Batch size

Plastic beaker:

  • 1-5 wafer of 4" at a time

PP-bath:

  • 1-25 wafers of 4" at a time

BHF-bath in cleanroom 3:

  • 1-25 wafers of 4" at a time

BHF-bath in cleanroom 4:

  • 1-25 wafers of 4" or 6" at a time

BHF-bath in RCA bench:

  • 1-25 wafers of 4" or 6" at a time

Plastic beaker:

  • 1-5 wafer of 4" at a time

PP-bath:

  • 1-25 wafers of 4" at a time

HF-bath in RCA bench:

  • 1-25 wafers of 4" or 6" at a time

1-7 wafer of 4" at a time

1-25 wafer of 4" at a time

Size of substrate

4"-6" wafers

2"-6" wafers

4" wafers

4" wafers

Allowed materials

In plastic beaker or PP-bath in the fume hood in cleanroom 2:

  • All materials

BHF-bath in cleanroom 3:

  • Silicon
  • Silicon nitrides
  • Silicon oxides
  • Photoresist

BHF-bath in the RCA bench:

  • Only wafers with phosphor glass or boron glass that comes directly from one of the furnaces in stack A.

In plastic beaker or PP-bath in the fume hood in cleanroom 2:

  • All materials

HF-bath in RCA bench:

  • Only wafers that are being RCA cleaned

In plastic beaker in the fume hood in cleanroom 2:

  • All materials
  • Silicon
  • Silicon nitrides
  • Silicon oxides
  • Photoresist

Life time of the photoresist and blue film in BHF

Photoresist delaminates from the substrate in BHF. For standard photoresist this process starts after about or less than ½ hour but the time can vary with resist pattern. It starts by under etching the photoresist at the edges. The life time can be prolonged a little to ½ hour - 40 minutes if the photoresist is baked at 120oC.

Blue film also has a limited life time in BHF. Blue film is mainly used for back side protecting the wafer while etching on the front side. The life time of Blue film is also about ½ hour.


KOH etching baths

THIS PAGE IS UNDER CONSTRUCTION



Equipment KOH3 KOH2 KOH1 KOH Fumehood
Purpose Wet etch of Silicon
  • Etch of Silicon in 28 wt% KOH
  • Etch of Silicon in 28 wt% KOH
  • Etch of Silicon in 28 wt% KOH saturated with IPA
  • Etch of Silicon in user mixed KOH
Link to safety APV and KBA
Performance Etch rates in crystalline silicon (100)
  • 0.4 µm/min (60 °C)
  • 0.7 µm/min (70 °C)
  • 1.3 µm/min (80 °C)
  • 0.4 µm/min (60 °C)
  • 0.7 µm/min (70 °C)
  • 1.3 µm/min (80 °C)
  • 0.7 µm/min (70 °C)
  • 0.2 µm/min (70 °C) for Boron doped Si (doping level > 5x1019 cm-3)
  • Somewhat lower than in the dedicated baths. Approximately 1 µm/min @ 80 °C in 28 wt%
Etch rates in Thermal SiO2
  • Theoretical values:
  • 1.2 nm/min (60 °C)
  • 6 nm/min (80 °C)
  • Theoretical values:
  • 1.2 nm/min (60 °C)
  • 6 nm/min (80 °C)
Roughness
  • Typical: 100-600 Å
  • Typical: 100-600 Å
  • May form hillocks (pyramidal)
  • Typical worse than KOH2 and KOH3
Anisotropy
  • The etch rate is very dependent on the crystal orientation of the silicon.
  • The etch rate is very dependent on the crystal orientation of the silicon.
  • With IPA some crystal planes etches at a slower rate than for KOH without IPA.
  • The etch rate is very dependent on the crystal orientation of the silicon.
Process parameter range Temperature
  • Max 80 °C (standard etch)
  • Max 80 °C (standard etch)
  • Max 70 °C if IPA added
  • Max 80 °C
Chemical solution
  • 28 wt% mixed in the ratio

KOH:H2O - 500 g : 1000 ml

  • 28 wt% mixed in the ratio

KOH:H2O - 500 g : 1000 ml

  • 28 wt% mixed in the ratio

KOH:H2O:IPA - 500 g : 1000 ml : ?? ml

  • Custom made
Substrates Batch size
  • 1-25 wafers at a time
  • 1-25 wafers at a time
  • 1-25 wafers at a time
  • 1-7 wafers at a time
Size of substrate
  • 4” wafers
  • 6” wafers
  • 4” wafers
  • 4” wafers
  • 2” wafers
  • 4” wafers
  • Small pieces
Allowed materials
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • All except for Polymers
Masking material
  • Stoichiometric Si3N4
  • Silicon rich nitride SiN
  • PECVD Si3N4
  • Thermal SiO2
  • Stoichiometric Si3N4
  • Silicon rich nitride SiN
  • PECVD Si3N4
  • Thermal SiO2
  • Stoichiometric Si3N4
  • Silicon rich nitride SiN
  • PECVD Si3N4
  • Thermal SiO2
  • Stoichiometric Si3N4
  • Silicon rich nitride SiN
  • PECVD Si3N4
  • Thermal SiO2