Process A specifications
Parameter Specification Average result
Etch rate (µm/min) Not specified 18.9
Etched depth (µm) 150 189.1
Scallop size (nm) < 800 718
Profile (degs) 91 +/- 1 91.1
Selectivity to AZ photoresist > 150 310
Undercut (µm) <1.5 0.84
Uniformity (%) < 3.5 3.0
Repeatability (%) <4 0.43



Process D recipe
Main etch (D->E) Etch Dep
Gas flow (sccm) SF6 275 O2 5 C4F8 150
Cycle time (secs) 2.4 2.0
Pressure (mtorr) 26 20
Coil power (W) 2500 2000
Platen power (W) 35 0
Cycles 110 (process time 08:04)
Common Temperature 0 degs, HBC 10 torr, Long funnel, with baffle & 100 mm spacers