Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142-pxnano2

From LabAdviser
Revision as of 11:32, 19 May 2011 by Jml (talk | contribs) (New page: == nano1.42 versus pxnano2 == {| border="2" cellpadding="2" cellspacing="1" |+ '''Recipe Sinano3.31''' |- ! rowspan="6" align="center"| Recipe | Gas | BCl<sub>3</sub> 5 sccm, HBR 15 sccm...)
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)

nano1.42 versus pxnano2

Recipe Sinano3.31
Recipe Gas BCl3 5 sccm, HBR 15 sccm
Pressure 2 mTorr, Strike 3 secs @ 5 mTorr
Power 900 W CP, 75 W PP
Temperature 50 degs
Hardware 100 mm Spacers
Time 60, 120 and 180 secs
Conditions Run ID 452, 453 and 454
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask 190 nm zep