Recipe nano1.3
Recipe Gas C4F8 38 sccm, SF6 52 sccm
Pressure 4 mTorr, Strike 3 secs @ 15 mTorr
Power 600 W CP, 40 W PP
Temperature -10 degs
Hardware 100 mm Spacers
Time 60 secs (a) and 120 secs (b)
Conditions Run ID (a) 1856 and (b) 1856+1857
Conditioning Sequence: Oxygen clean, processes, no oxygen between runs
Mask 190 nm zep