The slow etch
This work is done by Berit Herstrøm @DTU Nanolab, is nothing else is stated
The slow etch is designed to etch slow at low powers to etch thin films and to avoid overheating of samples mounted on a carrier with Capton/polyimide tape
Parameter
|
Recipe name: Slow Etch
|
Recipe name: Slow Etch2
|
Coil Power [W]
|
350
|
200
|
Platen Power [W]
|
25
|
50
|
Platen temperature [oC]
|
20
|
20
|
H2 flow [sccm]
|
15
|
15
|
CF4 flow [sccm]
|
30
|
30
|
Pressure [mTorr]
|
3
|
10
|
Typical results
|
Slow Etch
|
Slow Etch2
|
Etch of SRN
|
~43nm/min [measured 39-50 nm/min over a 6" wafer]
|
23-25 nm/min [4" on carrier]]
|
Etch rate of Si3N4
|
~49 nm/min [4" on carrier]
|
24-26 nm/min [4" on carrier]
|
Etch rate of SiO2
|
~42nm/min [41-43 nm/min over a 6" wafer]
|
13.7-14.7 nm/min [4" on carrier]
|
Etch rate in Si
|
ñm/min
|
11-13 nm/min (10% load, 4" wafer on 6" carrier)
|
Etch rate of Mir resist
|
~nm/min
|
~17 nm/min
|
Tested etch time without burning the resist
|
3 min (6 min => resist burned)
|
30 min
|
Profile [o]
|
|
|
Etch Profile SEM images
- Profile of etch for 'Slow Etch2' 12 min, 100mm wafer on 150mm carrier with double side polyimide tape (capton), Si3N4 from LPCVD
-
-
-
Etch Uniformity maps
- Map of etch rate measurements for 'Slow Etch2'
-
Etch rate map of Si3N4 etch on 4" wafer (on 6" carrier)
-
Etch rate map of SRN etch on 4" wafer (on 6" carrier)
-
Etch rate map of SiO2 etch on 4" wafer (on 6" carrier)
-
Etch rate map of Si etch on 4" wafer (on 6" carrier)
Test section - do not use