Germanium can be deposited by thermal evaporation, e-beam evaporation, and sputtering.
Thermal deposition
Ge deposition equipment comparison
| Thermal evaporation (Wordentec) | E-beam evaporation (Physimeca) | E-beam evaporation (Temescal) | Sputtering (Lesker) | Sputtering (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) | |
|---|---|---|---|---|---|
| General description | Thermal deposition of Ge | E-beam deposition of Ge | E-beam deposition of Ge | Sputter deposition of Ge | Sputter deposition of Ge |
| Pre-clean | RF Ar clean | - | Ar ion beam clean | RF Ar clean | RF Ar clean |
| Layer thickness | 10Å to about 2000Å (in total distributed on all loaded wafers) | 10Å to about 3000Å | 10Å to about 1000 nm | 10Å to at least 1000 Å | 10Å to ? |
| Deposition rate | From 0.4 Å/s up to about ~2Å/s | 5 Å/s | From 1 Å/s up to 5 Å/s | Depends on deposition parameters | Depends on deposition parameters |
| Batch size |
Many small pieces |
|
|
smaller pieces |
|
| Allowed substrates |
|
|
|
|
|
| Allowed materials |
|
|
|
|
|
| Comment | Recommended for unexposed e-beam resist |