Specific Process Knowledge/Thin film deposition/Deposition of Carbon
We can deposit Carbon (C) by DC sputtering in Sputter-System (Lesker). A 2-inch target from gun 1 (DC) is used in the process. Since the material is known to possess cross-contamination issues it was decided to cover all other guns with the protection foil.
The fabrication and characterization described below were conducted in 2022 by Patama Pholprasit and Evgeniy Shkondin, DTU Nanolab. The prepared samples were investigated by the X-ray Reflectivity (XRR), Spectroscopi Ellipsometry (SE), Photo Electron Spectroscopy (XPS), Scanning Electron Microscopy (SEM), and Graizing Incident Diffraction (GiXRD) methods. The focus of the study was the deposition conditions.
Recipe:
- Power: 200 W
- Pressure: 3 mTorr
- Power rump: 0.3 W/s
- Deposition mode: DC (Src1)
- Deposition time: 10, 20, 30 min and 6000s for GiXRD measurement)
- Substrate: 4-inch Si and a variety of others (glass, silicon nitride) to study adhesion and conductivity.
Deposition Rate
Deposition rate for C at 200W power (DC) and 3 mTorr presssure is 0.01 nm/s
-
Carbon thin films deposited on Si wafer and measured by XRR method. 10, 20 and 30 min of deposition time using 200W, 3 mTorr, Src1 DC.
X-ray Reflectivity
X-ray analysis (XRR) of samples (deposited at 10min, 20 min, and 30 min) have been performed to investigate the thicknesses, roughness, and density profiles.
The scans has been obtained using Rigaku XRD SmartLab equipment. The voltage and current settings for the Cu X-ray tube were standard 40kV and 30mA. The incident optics contained a IPS (incident parallel slit) adaptor with 5 ° Soller slit. Other slits: IS=0.03mm RS1=0.03mm and RS2=0.075mm. Step size: 0.01 and measurement time - 5s for each point. Fitting procesure was performed using commercial GlobalFit software assuming the model based on Si or SiO2 substrates with native oxide/interlayer followed by the deposited C film with thin oxides and moisture surfaces. The results are summarized in a tables below.
Fitting resilts for Carbon films
-
10 min deposition from Src1.
-
20 min deposition from Src1.
-
30 min deposition from Src1.
XRR results for Carbon layers | ||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
|
Fitting parameters | |||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Sample | Moisture | Carbon | Si native oxide | Si substrate | Fitting parameters | ||||||||
Delta | Beta | Delta | Beta | Delta | Beta | Delta | Beta | Intensity | Background | Fitting area () | R | ||
10 min | 1.3932E-6 | 3.2352E-8 | 6.4587E-6 | 9.7010E-9 | 6.9134E-6 | 1.6054E-7 | 7.5860E-6 | 1.7616E-7 | 1.14309 | 7.02370E-8 | 0.2666 - 5.000 | 0.02092 | 0.01081 |
20 min | 1.4031E-6 | 3.2581E-8 | 6.4279E-6 | 9.6547E-9 | 7.1423E-6 | 1.6585E-7 | 7.5860E-6 | 1.7616E-7 | 0.93079 | 1.96097E-8 | 0.2666 - 4.000 | 0.01987 | 0.00899 |
30 min | 1.2905E-6 | 2.9968E-8 | 6.4412E-6 | 9.6747E-9 | 6.4832E-6 | 1.5055E-7 | 7.5860E-6 | 1.7616E-7 | 0.88610 | 3.11353E-8 | 0.3143 - 4.000 | 0.02722 | 0.01877 |
Graizing Incident Diffraction (GiXRD)
Graizing Incident Diffraction (GiXRD) of 60 nm C sample (deposited at 6000s, 200W, 3 mTprr, DC, Src1) has been performed to investigate the phase profile. The analysis revealed the amorphous film.
The scan has been obtained using Rigaku XRD SmartLab equipment. The voltage and current settings for the Cu X-ray tube were standard 40kV and 30mA. The incident optics contained a IPS (incident parallel slit) adaptor with 5 ° Soller slit. Other conditions: IS=1 mm, ω=2 ° PSA 0.5 ° RS1=RS2=open, Lenght-limiting slit=15mm, Speed: 0.5 ° /min. Angle range: 20-90 2θ.
-
Amorphous film. No diffraction peaks.
X-ray Photoelectron Spectroscopy
Oxygen is almost non existing in the film (around or less than 1 at.%). The signal eventually rises during the depth profiling. It comes from the Carbon-Silicon interface (native oxide). No other contaminants have been found.
-
Atomic concentartion as a fnction of depth. Etching parameters: 1000eV, low current, 10s@50 levels.
-
Survey spectrum after 10s Ar+ etch (1000eV, low current).
-
C 1s.
-
O 1s.
-
Si 2p.
-
2D image of XPS depth profiles.
Scanning Electron Microscopy
-
C deposited on high aspect ratio silicon structure (trenches) with 200W power and 3 mTorr, 20min. Cross-sectional tilted view.
Spectroscopic Ellipsometry
Results have been obtained for Si wafers with native oxide, based on ellipsometry study. The Bspline model has been used for analysis.
-
Refractive index of carbon deposited at 30 min, 200W, 3 mTorr, DC, Src1.
-
Absorption coefficient of carbon deposited at 30 min, 200W, 3 mTorr, DC, Src1.
Conductivity
Sheet resistance has been performed using Four point probe – Jandel. The deposited carbon film (6nm at 600s, 200W, 3 mTorr) on top of a microscope glass slide showed 178-223 MOhm/sq range.
Deposition Recordings
-
Ar flow recording. Thin layer (1800s deposition time).
-
Pressure recording. Thin layer (1800s deposition time).
-
Power recording. Thin layer (1800s deposition time).
-