Specific Process Knowledge/Thin film deposition/Deposition of Titanium
Feedback to this page: click here
Titanium deposition
Titanium can be deposited by e-beam evaporation. In the chart below you can compare the different deposition equipment.
E-beam evaporation (Alcatel) | E-beam evaporation (Wordentec) | E-beam evaporation (PVD co-sputter/evaporation) | E-beam evaporation (Physimeca) | Sputter deposition (Wordentec) | Sputter deposition (Lesker) | E-beam evaporation (III-V Dielectric evaporator) | |
---|---|---|---|---|---|---|---|
General description | E-beam deposition of Titanium | E-beam deposition of Titanium | E-beam deposition of Titanium | E-beam deposition of Titanium | Sputter deposition of Titanium | Sputter deposition of Titanium | E-beam deposition of Titanium |
Pre-clean | RF Ar clean | RF Ar clean | RF Ar clean | RF Ar clean | RF Ar clean | ||
Layer thickness | 10Å to 1µm* | 10Å to 1 µm* | 10Å to 2000Å | 10Å to 1000Å | . | . | 10Å to 1000Å |
Deposition rate | 2Å/s to 15Å/s | 10Å/s to 15Å/s | About 1Å/s | About 10Å/s | Depending on process parameters, see here. | Depending on process parameters, about 1 Å/s. | About 1Å/s |
Batch size |
|
|
|
|
|
|
|
Allowed substrates |
|
|
|
|
|
|
|
Allowed materials |
|
|
|
|
|
|
|
Comment | Only very thin layers (up to 100nm). |
* For thicknesses above 200 nm permission from ThinFilm group (thinfilm@danchip.dtu.dk) is required.
Comments: Choise of equipment
Comments: Adhesion layer
Ti as adhesion layer
Titanium is most often used as a adhesion layer for other metals, like for example gold. Gold does not stick very well to Si, and to prevent it to come off in future process steps or in the final application, a layer of Ti (or Cr) is often deposited onto the wafer.
The most common thickness of the Ti adhesion layer is 10 nm. Also layers with a thickness of 5 nm is used.
Very thin adhesion layers
If it is important to have a very thin Ti layer, it is possible to use even thinner adhesion layers. There are some experiences of using a 3 nm Ti as adhesion layer for a 200 nm thick gold layer. In this case a Si wafer was dipped in buffer and rinsed in water immediately before being placed in the PVD equipment (Wordentec). After a RF clean process of the wafer, 3nm of Ti and 200 nm of Au was deposited, and this worked fine during futher processing.