Chromium etch in ICP metal

The Chromium etch has ONLY been carried out on the following substrate stack: The Chromium is sputter deposited onto a 2" quartz wafer and pattered by e-beam with Zep520A resist. This 2" QZ wafer is bonded with crystal bond to a 65mmx65mm quartz plate with the thickness: 6.35mm. This QZ plate is bonded to a Si wafer.

Cr etch by bghe@danchip
Parameter Cr etch
Cl2 (sccm) 65
O2 (sccm) 15
Pressure (mTorr) 15
Coil power (W) 300
Platen power (W) 15
Temperature (oC) 50 (no back side cooling)
Spacers (mm) 100
Etch rate (nm/min) ~14
Zep520A resist selectivity ~0.9
Comment .