Specific Process Knowledge/Thin film deposition/Deposition of Silicon
Feedback to this page: click here
PolySilicon can be sputtered in Alcatel and be deposited in the PolySilicon furnace. In the chart below you can compare the two different deposition methodes:
Sputter (Alcatel) | Sputter(PVD co-sputter/evaporation) | Furnace PolySi (Furnace LPCVD pSi) | Sputter (Wordentec) | |
---|---|---|---|---|
Batch size |
|
|
|
|
Pre-clean | RF Ar clean | RF Ar clean | RCA clean for wafers that are not fresh form the box. | RF Ar clean |
Layer thickness | 10Å to 1µm | 10Å to about 3000Å | ~50Å to 2µm, if thicker layers are needed please ask the furnace team. | 10Å to about 3000Å |
Deposition rate | 2Å/s to 15Å/s | Dependent on process parameters, but in the order of 1 Å/s. See more here |
|
Dependent on process parameters, but in the order of 1 Å/s. See more here. |
Process temperature | ? | Option: heating wafer up to 400 deg C | 560 oC (amorph) and 620 oC (poly) | ? |
Step coverage | Poor | . | Good | .
|
Adhesion | Bad for pyrex, for other materials we do not know | . | Good for fused silica, silicon oxide, silicon nitride, silicon | . |
Substrate material allowed | Pyrex, fused silica, silicon, metals, oxide, nitride, blue tape | Pyrex, fused silica, silicon, metals, oxide, nitride | Fused silica, Silicon, oxide, nitride | Pyrex, fused silica, silicon, metals, oxide, nitride
|
Doping facility | None | None | Can be doped during deposition with Boron and/or Phosphorous | None |
Sputtered Silicon in the Alcatel
The parameter(s) changed | New value(s) | Deposition rate |
---|---|---|
Standard parameters | None | |
Power | 400W | 3.8 Å/s |
Sputtered Silicon in the PVD co-sputter/evaporation
See this page: Si sputter in PVD co-sputter/evaporation
Sputtered Silicon in Wordentec
See this page: Si sputter in Wordentec