Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300/IBE magnetic stack etch

From LabAdviser

Process parameters for the acceptance test

Parameter Ti etch acceptance
Neutalizer current [mA] 450
RF Power [W] 800
Beam current [mA] 400
Beam voltage [V] 500
Beam accelerator voltage 500
Ar flow to neutralizer [sccm] 5.0
Ar flow to beam [sccm] 10.0
Rotation speed [rpm] 20
Stage angle [degrees] 5
Helium backside cooling [Torr] 37.5

Some SEM profile images of the etched stacks

Magnetic stack of Ta/MnIr/NiFe/Ta/Tao/Ta/MnIr/NiFe/Ta. Redeposition of etched material at photo resist. Profile ~78°
Etched magnetic stack with pool structure transfer. Chosen etch parameters result in severe footing
Etched magnetic stack with pool structure transfer. Chosen etch parameters result in severe trenching