Specific Process Knowledge/Thin film deposition/Deposition of Silicon
PolySilicon can be sputtered in Alcatel and be deposited in the PolySilicon furnace. In the chart below you can compare the two different deposition methodes:
Sputter (Alcatel) | Sputter(PVD co-sputter/evaporation) | Furnace PolySi | Sputter (Wordentec) | ||
---|---|---|---|---|---|
Batch size |
|
|
|
. |
|
Pre-clean | RF Ar clean | RF Ar clean | RCA clean for wafers that are not fresh form the box. | RF Ar clean | |
Layer thickness | 10Å to 1µm | 10Å to about 3000Å | ~50Å to 2µm, if thicker layers are needed please ask the furnace team. | Thin layers | |
Deposition rate | 2Å/s to 15Å/s | Dependent on process parameters, but in the order of 1 Å/s. See more here |
|
Dependent on process parameters, but in the order of 1 Å/s. See more here | |
Process temperature | ? | Option: heating wafer up to 400 deg C | 560 oC (amorph) and 620 oC (poly) | ? | |
Step coverage | Poor | . | Good | ||
Adhesion | Bad for pyrex, for other materials we do not know | . | Good for fused silica, silicon oxide, silicon nitride, silicon | ||
Substrate material allowed | Pyrex, fused silica, silicon, metals, oxide, nitride, blue tape | Pyrex, fused silica, silicon, metals, oxide, nitride | Fused silica, Silicon, oxide, nitride | ||
Doping facility | None | None | Can be doped during deposition with Boron and/or Phosphorous |
|
Sputtered Silicon in the Alcatel
The parameter(s) changed | New value(s) | Deposition rate |
---|---|---|
Standard parameters | None | |
Power | 400W | 3.8 Å/s |
Sputtered Silicon in the PVD co-sputter/evaporation
See this page: Si sputter in PVD co-sputter/evaporation