Etching of nanostructures in silicon using the ICP Metal Etcher

Sinano3.0 Sinano3.1 Sinano3.2 Sinano3.3 Sinano3.4 Sinano4.0 Sinano3.5 Sinano3.6
Cl2 (sccm) 0 0 0 0 0 20 15 15
BCl3 (sccm) 5 3 5 5 5 0 5 5
HBr (sccm) 15 17 15 15 15 0 0 0
Coil power (W) 900 (Load) 900 (Forward) 900 (Forward) 900 (Forward) 900 (Forward) 900 (Load) 900 (Load) 900 (Forward)
Platen power (W) 50 50 60 75 90 60 60 60
Pressure (mtorr) 2 2 2 2 2 2 5 10
Process time (s) 150 180 120 180 120 90 120 180