Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF)

From LabAdviser

Wet Silicon Oxide Etch (BHF and SIO Etch (wetting agent))

 
Wet Silicon Oxide Etch (BHF): positioned in cleanroom 3

Silicon oxide can be etched using HF. At Danchip it is mainly used in a buffered version BHF (premixed). The BHF has a more stable etch rate and more gentle to photoresist due to an almost pH neutral solution which makes photoresist a good masking material for the oxide etch.

SIO etch (BHF with wetting agent) can also be used for etching silicon oxide. This is mainly for etching small holes. If you have wetting problems in BHF try the SIO etch. It is also a good idea to wet the sample in water before etching.


Silicon oxide etch data

BHF 5% HF SIO
General description

Etching of silicon oxide with a stable etch rate

Mainly for removing native oxide

Etching of silicon oxide - especially for etching small holes

Chemical solution BHF 5% HF BHF with wetting agent
Process temperature Room temperature Room temperature Room temperature
Possible masking materials
  • Photoresist
  • Silicon nitride
  • PolySi
  • Blue film

In beaker or PP-bath in the fume hood in cleanroom 2:

  • All materials

In RCA bench:

  • Only new wafers from the box or during RCA cleaning
  • Photoresist
  • Silicon nitride
  • PolySi
  • Blue film
Etch rate
  • Wet thermal oxide:~80nm/min
  • PECVD1 (standard):~147nm/min
  • TEOS:~265nm/min
  • Wet thermal oxide:~25nm/min
  • PECVD1 (standard):~87nm/min
  • TEOS:~153nm/min
  • Wet thermal oxide:~80nm/min
  • PECVD1 (standard):~147nm/min
  • TEOS:~265nm/min
Selectivity RSi3N4 / RSiO2 ~21 <21
Batch size

1-25 wafers at a time

1-25 wafer at a time

Size of substrate

2-6" wafers

2-6" wafers

Allowed materials
  • Silicon
  • Silicon nitrides
  • Silicon oxides
  • Silicon
  • Silicon nitrides
  • Silicon oxides
 
SIO etch (BHF with wetting agent): positioned in cleanroom 4