Specific Process Knowledge/Etch/KOH Etch

From LabAdviser

KOH etch - Anisotropic silicon etch

KOH etch for 4" wafers: positioned in cleanroom 3

KOH belongs to the family of anisotropic Si-etchants based on aqueous alkaline solutions. The anisotropy stems from the different etch rates in different crystal directions. The {111}-planes are almost inert whereas the etch rates of e.g. {100}- and {110}-planes are several orders of magnitude faster.

KOH-etching is a highly versatile and cheap way to realize micromechanical structures if you can live with the necessary SiFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _3} NFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _4} - or SiOFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2} masking materials and the K contamination of the surface. The latter necessitates in most cases a wet post-clean ('7-up' or RCA-clean) if the wafer is to be processed further.

At Danchip we use as a standard a 28 wt% KOH. The etch rate - and the selectivity towards a SiOFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2} -mask - is depending on the temperature. We normally use T=80 oC but may choose to reduce this to e.g. 60 oC or 70 oC in case of a high-precission timed etch (e.g. defining a thin membrane). In some cases we recommend to saturate the standard 28 wt% KOH with IPA with an etch temperature at T=70 oC (reduce evaporation of IPA). One example is for boron etch-stop, where the selectivity towards the boron-doped silicon is improved roughly a factor of 10 compared to the standard etch. Key facts for the two solutions are resumed in the table:


Comparing the two solutions

28 wt% KOH 28 wt% KOH sat. with IPA
General description

Etch of Si(100)

Etch of Si(100) with boron etch-stop

Chemical solution KOH:HFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2} O 500 g : 1000 ml KOH:HFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2} O:IPA 500 g : 1000 ml : ?? ml
Process temperature 60 oC

70 oC

80 oC

20 oC
Possible masking materials:

Photoresist (1.5 µm AZ5214E)

Photoresist (1.5 µm AZ5214E)

Etch rate

~100 nm/min (Pure Al)

~60(??) nm/min

Batch size

1-25 wafers at a time

1-25 wafer at a time

Size of substrate

4" wafers

4" wafers

Allowed materials
  • Aluminium
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resist
  • Aluminium
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resist