Specific Process Knowledge/Etch/Etching of Gold

From LabAdviser

Etching of Gold

Etching of Gold is done wet at Danchip. We have two different solutions:

  1. KI:IFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2} :HFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2} O - 400g:100g:400ml?
  2. HNOFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _3} :HCl - 1:3


Comparing the two solutions

Iodine based gold etch Aqua Regia (Kongevand)
General description

Etch of pure Gold

Etch of pure Gold

Chemical solution KJFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle J} :JFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2} :HFailed to parse (SVG (MathML can be enabled via browser plugin): Invalid response ("Math extension cannot connect to Restbase.") from server "https://wikimedia.org/api/rest_v1/":): {\displaystyle _2} O<math> 100g:25g:500ml
Process temperature 50 oC 20 oC
Possible masking materials:

Photoresist (1.5 µm AZ5214E)

Photoresist (1.5 µm AZ5214E)

Etch rate

~100 nm/min (Pure Al)

~60(??) nm/min

Batch size

1-25 wafers at a time

1-25 wafer at a time

Size of substrate

4" wafers

4" wafers

Allowed materials
  • Aluminium
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resist
  • Aluminium
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • E-beam resist