Silicon oxide can be etched using either wet chemistry or dry etch equipment. Wet chemistry is mainly used to remove all the oxide on the surface (backside and front side) of a wafer or for isotrotropic etching. Dry etching etches anisotropic. It etches one side of the wafer at a time and can be used to etch structures with several masking materials.
Etch of silicon oxide can be done by either wet etch or dry etch. The standard setups for this here at DANCHIP are:
===Wet etches:===
*[[Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF)|Wet Silicon Oxide Etch]]
===Dry etches:===
*[[/SiO2 etch using RIE1 or RIE2|Dry etch using RIE1 or RIE2]]
*[[/SiO2 etch using AOE|Dry etch using AOE]]
*[[Specific Process Knowledge/Etch/IBE/IBSD Ionfab 300|IBE/IBSD Ionfab 300]]
==Comparison of wet Silicon Oxide etch and dry etches (RIE and AOE) etch for etching of Silicon Oxide==
{| border="2" cellspacing="0" cellpadding="4" align="center"
!
! Wet Silicon Oxide etch (BHF, SIO Etch (wetting agent), 5%HF)
! RIE
! AOE
|- valign="top"
|'''General description'''
|
*Isotropic etch
|
*Anisotropic etch: vertical sidewalls
|
*Anisotropic etch: vertical sidewalls, especially good for deep etch and high aspect ratio etch
|-valign="top"
|'''Possible masking materials'''
|
*Photoresist
*Silicon nitride
|
*Photoresist
*(Poly)Silicon
*Aluminium
*Other metals that covers less the 5% of the wafer area (ONLY RIE2!)
|
*Photoresist
*(Poly)Silicon
*Aluminium
*Chromium (ONLY if the other masking materials can not be used!)
|- valign="top"
|'''Etch rate'''
|
*~75 nm/min (Thermal oxide) in BHF
*~90 nm/min (Thermal oxide) in SIO Etch
*~25 nm/min (Thermal oxide) in 5%HF
|
*Typically 40-120 nm/min can be increased or decreased by using other recipe parameters. 
|
*Typically 200-600 nm/min can be increased or decreased by using other recipe parameters.
|-valign="top"
|'''Batch size'''
|
*1-25 wafers at a time
|
*1 wafer at a time
|
*1 wafer at a time
|-valign="top"
|'''Size of substrate'''
|
*4" wafers
|
*4" wafers or smaller pieces
|
*6" or 4" depending on the setup (smaller pieces if you have a carrier wafer)
|-valign="top"
|'''Allowed materials'''
|
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*Blue film
*Gold (Au) and Nickel (Ni) (but only in BHF2 (KOH)!)
|
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*E-beam resist
*Aluminium
*Other metals that covers less the 5% of the wafer area (ONLY RIE2!)
|
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*E-beam resist
*Aluminium
*Chromium (ONLY as masking material if the other masking materials can not be used!)
|-
|}
=This Part is under construction=
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide click here]'''
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide click here]'''
<!-- Replace "http://labadviser.danchip.dtu.dk/..." with the link to the Labadviser page-->
<!-- Replace "http://labadviser.danchip.dtu.dk/..." with the link to the Labadviser page-->

Revision as of 12:13, 13 May 2013

Feedback to this page: click here

Comparing silicon oxide etch methods at Danchip

There are a broad varity of silicon oxide etch methods at Danchip. The methodes are compared here to make it easier for you to compare and choose the one that suits your needs.


Compare the methods for Silicon Oxide etching

Wet Silicon Oxide etch (BHF/HF) RIE (Reactive Ion Etch) AOE (Advanced Oxide Etch) IBE/IBSD Ionfab 300
Generel description
  • Isotropic etch
  • Anisotropic etch: vertical sidewalls
  • Anisotropic etch: vertical sidewalls
  • Primarily for pure physical etch by sputtering with Ar-ions
Possible masking materials
  • Photoresist
  • PolySilicon
  • Silicon nitride (LPCVD)
  • Blue film
  • Cr/Au for deeper etches (plastic beaker)
  • Photoresist
  • DUV resist
  • E-beam resist
  • Silicon Oxide
  • Silicon Nitride
  • Metals if they cover less than 5% of the wafer area (ONLY RIE2!)
  • Photoresist
  • DUV resist
  • E-beam resist
  • Silicon Oxide
  • Silicon Nitride
  • Aluminium
  • Chromium (Please try to avoid this)
  • Any material that is accepted in the machine
Etch rate range
  • ~75 nm/min (Thermal oxide) in BHF
  • ~90 nm/min (Thermal oxide) in SIO Etch
  • ~25 nm/min (Thermal oxide) in 5%HF
  • ~3-4µm/min in 40%HF
  • Process dependent
  • Tested range: ~20nm/min - ~120nm/min
  • Process dependent
  • Tested range: ~230nm/min - ~550nm/min
  • Process dependent
  • Tested once ~22nm/min
Substrate size
  • #1-25 100mm wafers in our 100mm bath
  • What can be fitted in a plastic beaker
  • As many small samples as can be fitted on the 100mm carrier.
  • #1 100mm wafer (or smaller with carrier)
  • #1 150mm wafer (only RIE2 when set up for 150mm)
  • As many small samples as can be fitted on a 100mm wafer
  • #1 50 mm wafer fitted on a 100mm wafer
  • #1 100 mm wafer
  • #1 150 mm wafers (only when the system is set up to 150mm)
  • As many samples as can be securely fitted on a up to 200mm wafer
  • #1 50 mm wafer with special carrier
  • #1 100 mm wafer with special carrier
  • #1 150 mm wafers with special carrier
  • #1 200 mm wafer
Allowed materials

In the dedicated bath:

  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • Blue film

In a plastic beaker:

  • No limits cross contamination wise
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • DUV resist
  • E-beam resist
  • Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)
  • Quartz/fused silica
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • DUV resist
  • E-beam resist
  • Aluminium
  • Chromium (try to avoid it)
  • Quartz/fused silica
  • Silicon
  • Silicon oxides
  • Silicon (oxy)nitrides
  • Metals from the +list
  • Metals from the -list
  • Alloys from the above list
  • Stainless steel
  • Glass
  • III-V materials
  • Resists
  • Polymers
  • Capton tape