Jump to content

Specific Process Knowledge/Characterization/KLA-Tencor Surfscan 6420: Difference between revisions

From LabAdviser
Mdyma (talk | contribs)
Mdyma (talk | contribs)
Line 1: Line 1:
=<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]=
'''Feedback to this page''': '''[mailto:characterization@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Characterization/KLA-Tencor_Surfscan_6420&action=edit&redlink=1 click here]'''
'''Feedback to this page''': '''[mailto:characterization@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Characterization/KLA-Tencor_Surfscan_6420&action=edit&redlink=1 click here]'''



Revision as of 12:05, 3 May 2013

Feedback to this page: click here

KLA-Tencor Surfscan 6420

The image is from the cleanroom at the place it was refurbish in California.

Particles counting of a unpatterned surface. A broad range of particles size from 0.1 µm to greater than 3 µm can be measured on a polished silicon or epitaxial layers. Thin films as e.g. Poly-si, Nitride and thermal Oxide can also be inspected. The system will remove small surface roughness so it not count as a particle.



Overview of the performance of the Surfscan 6420 and some process related parameters

Purpose
  • Particles counting
Performance Particles size
  • 0.1 µm to 3 µm
Througput
  • Up to 100 wafer per hour (200 mm)
Repeatbility
  • Within 1%, 1σ (mean count > 500, 0,204 µm diameter latex spheres)
Process parameter range Process Temperature
  • Room temperature
Process pressure
  • 1 atm
Substrates Batch size
  • Small wafer pieces can all be used
  • 1-25 100 mm wafers
  • 1-25 150 mm wafers
  • 1-25 200 mm wafers
Substrate material allowed