Specific Process Knowledge/Etch/Wet Silicon Nitride Etch: Difference between revisions

From LabAdviser
Kb (talk | contribs)
BGE (talk | contribs)
No edit summary
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:wetchemistry@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Silicon_Nitride_Etch click here]'''


'''Feedback to this page''': '''[mailto:wetchemistry@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Silicon_Nitride_Etch click here]'''
'''Feedback to this page''': '''[mailto:wetchemistry@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Silicon_Nitride_Etch click here]'''

Revision as of 14:03, 7 March 2013

Feedback to this page: click here


Wet Silicon Nitride Etch

Wet nitride etch: positioned in cleanroom 4

Wet Etching of silicon nitride - stoichiometric and Si-rich - is done in a dedicated laminar flow bench with an integrated quartz tank (Tiger Tank - TT-4). The quartz tank can take up to one 6" wafer carrier. The flow bench is placed in cleanroom 4. The process is mainly used to strip silicon nitride (maskless), but can also be used for masked etching of silicon nitride using some kind of silicon oxide as etch mask. However, the wet silicon nitride etch is isotropic - meaning that the under-etching (etch-bias) at least amounts to the thickness of the silicon nitride layer.

The etch solution is initially 85 wt% H3PO4 which is heated up to the boiling temperature - ca. 157 oC. Water is allowed to boil off thus raising the concentration and the boiling temperature of the solution until a boiling temperature of 180 oC is reached. Thereafter, the wafers are submerged into the bath and the water-cooled lid is closed to maintain the concentration and the boiling temperature. In some cases a lower boiling temperature is chosen - typically 160 oC - which lowers the etch rate and improves the selectivity RSi3N4 / RSiO2.


NB: Great care has to be taken in this process due to risk of "shock-boiling"



Nitride Etch data

Nitride Etch @ 180 oC Nitride Etch @ 160 oC
General description

Etch/strip of silicon nitride

Etch/strip of silicon nitride

Chemical solution H3PO4 (85 wt%) H3PO4 (85 wt%)
Process temperature 180 oC 160 oC
Possible masking materials
  • Thermal oxide (converted si-rich surface)
  • LPCVD-oxide (TEOS)
  • PECVD-oxide
  • Thermal oxide (converted si-rich surface)
  • LPCVD-oxide (TEOS)
  • PECVD-oxide
Etch rate
  • ~85 Å/min (stoichiometric Si3N4)
  • ~60 Å/min (Si-rich Si3N4)
  • ~30 Å/min (annealed Si-rich Si3N4)
  • ~4 Å/min (Thermal oxide)
  • ~26 Å/min (Si-rich Si3N4)
Selectivity RSi3N4 / RSiO2 ~20 The selectivity (sirich nitride:oxide) is higher at 160 oC than at 180 oC
Batch size

1-25 wafers at a time

1-25 wafer at a time

Size of substrate

2-6" wafers

2-6" wafers

Allowed materials
  • Silicon
  • Silicon nitrides
  • Silicon oxides
  • Silicon
  • Silicon nitrides
  • Silicon oxides