Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300/IBE magnetic stack etch: Difference between revisions
No edit summary |
|||
| Line 79: | Line 79: | ||
|} | |} | ||
End point detection is achieved by SIMS, and the etch rate is approximately 25 Nm/min. | End point detection is achieved by SIMS, and the etch rate is approximately 25 Nm/min. | ||
Resist stripping can be hard due to burned resist, to remedy this try to lower the current. Changing the currect will chance the sidewall angle and new studies of etch profiles will be necessary. For help, discussion and further info please contact [mailto:kristian.rasmussen@nanotech.dtu.dk Kristian Hagsted Rasmussen]. | |||
===Problems with resists stripping af etching=== | |||
Resist stripping after the etch can be hard due to burned resist, to remedy this try to lower the current. Changing the currect will chance the sidewall angle and new studies of etch profiles will be necessary. For help, discussion and further info please contact [mailto:kristian.rasmussen@nanotech.dtu.dk Kristian Hagsted Rasmussen]. | |||
===Design of Experiment results=== | ===Design of Experiment results=== | ||
Revision as of 15:27, 6 February 2013
Results of Design of Experiments optimization of magnetic stack etching (Kristian Hagsted Rasmussen spring 2011)
Process parameters
To find the optimal parameters, Design of Experiments was applied with the intervals shown on the figure below. The final optimized recipe is listed in the table.
Some SEM profile images of the etched stacks
For a good pattern transfer with IBE a large amount of redeposition on the resist edge has been observed. To reduce this redeposition the best option seems to be to use a photo resist just thick enough for the wanted etch depth. An alternative is sidewall sputtering at low incident angle. However experiments have shown poor cleaning rate and for narrow structures low angles will give rise to shadowing effects.
Endpoint detection with SIMS
End point detection is achieved by SIMS, and the etch rate is approximately 25 Nm/min.
Problems with resists stripping af etching
Resist stripping after the etch can be hard due to burned resist, to remedy this try to lower the current. Changing the currect will chance the sidewall angle and new studies of etch profiles will be necessary. For help, discussion and further info please contact Kristian Hagsted Rasmussen.
Design of Experiment results
The etch rate and corner angle are dependent on several parameters each. Below two graphs showing these dependencies are shown. Note that the values are fitted and may not represent the actual value after etch, however feel free to use the graphs to estimate the values for your test run.
Conclusions
- Etch rate around 20 nm/min with optimized recipe.
- Good feature definition after etch.
- Good end point detection by SIMS.
- Burned resist: Lower current, 300 mA can limit resist burning. Note this will affect pattern transfer.
- Hare ears due to redeposition, thinner resist can limit the size.