Specific Process Knowledge/Etch/ASE (Advanced Silicon Etch): Difference between revisions
Appearance
No edit summary |
No edit summary |
||
| Line 5: | Line 5: | ||
The Bosch process uses alternation between an etch cycle and a passivation cycle. In the case of the silicon etching on the ASE, an etch phase with SF<sub>6</sub> and O<sub>2</sub> alternates with a passivation phase with C<sub>4</sub>F<sub>8</sub>. | The Bosch process uses alternation between an etch cycle and a passivation cycle. In the case of the silicon etching on the ASE, an etch phase with SF<sub>6</sub> and O<sub>2</sub> alternates with a passivation phase with C<sub>4</sub>F<sub>8</sub>. | ||
Two recipes have been optimized for the ASE. | Two recipes have been optimized for the ASE. Their specification is on a 10 % etch load wafer with trenches. | ||
* '''Shallolr''': The shallow etch process will etch a 2 <math>\mu</math>m | * '''Shallolr''': The shallow etch process will etch a 2 <math>\mu</math>m opening down to make a 20 <math>\mu</math>m trench. | ||
* '''Deepetch''': The deep etch process will etch a 50 <math>\mu</math>m | * '''Deepetch''': The deep etch process will etch a 50 <math>\mu</math>m opening down to make a 300 <math>\mu</math>m trench. | ||
{| border="2" cellpadding="2" cellspacing="1" align="left" | {| border="2" cellpadding="2" cellspacing="1" align="left" | ||
Revision as of 19:27, 25 November 2007
The ICP-DRIE (Inductively Coupled Plasma - Deep Reactive Ion Etcher) tool at Danchip is manufactured by STS and is called the ASE (Advanced Silicon Etcher). The main purpose of the ASE is etching of silicon using Bosch process.
The Bosch process:
The Bosch process uses alternation between an etch cycle and a passivation cycle. In the case of the silicon etching on the ASE, an etch phase with SF6 and O2 alternates with a passivation phase with C4F8.
Two recipes have been optimized for the ASE. Their specification is on a 10 % etch load wafer with trenches.
- Shallolr: The shallow etch process will etch a 2 m opening down to make a 20 m trench.
- Deepetch: The deep etch process will etch a 50 m opening down to make a 300 m trench.
| Common parameters | Multiplexed parameters | |||
|---|---|---|---|---|
| Parameter | Setting | Parameter | Etch | Passivation |
| Temperature | 10oC | SF6 Flow | 260 sccm | 0 sccm |
| No. of cycles | 31 | O2 Flow | 26 sccm | 0 sccm |
| Process time | 5:56 mins | C4F4 Flow | 0 sccm | 120 sccm |
| APC mode | manual | RF coil | 2800 W | 1000 W |
| APC setting | 86.8 % | RF Platen | 16 W | 0 W |
| Cycle time | 6.5 s | 5 s | ||
| Common parameters | Multiplexed parameters | |||
|---|---|---|---|---|
| Parameter | Setting | Parameter | Etch | Passivation |
| Temperature | 20oC | SF6 Flow | 230 sccm | 0 sccm |
| No. of cycles | 250 | O2 Flow | 23 sccm | 0 sccm |
| Process time | 54:10 mins | C4F4 Flow | 0 sccm | 120 sccm |
| APC mode | manual | RF coil | 2800 W | 1000 W |
| APC setting | 87.7 % | RF Platen | 19 W | 0 W |
| Cycle time | 8 s | 5 s | ||