Specific Process Knowledge/Etch/DRIE-Pegasus/processB: Difference between revisions
| Line 95: | Line 95: | ||
A number of wafers are patterned with the [[Specific Process Knowledge/Photolithography/masks/travka|travka masks]] in 4 microns of AZ photoresist. The wafers are then etc | A number of wafers are patterned with the [[Specific Process Knowledge/Photolithography/masks/travka|travka masks]] in 4 microns of AZ photoresist. The wafers are then etc | ||
{| | |||
{| | |||
| STYLE="vertical-align: top"| | |||
{| border = 1 | |||
|+ '''Wafers''' | |||
|- | |- | ||
! Wafer number | ! width="50" |Wafer number | ||
! Mask | ! width="50" |Mask | ||
! Process B duration | ! width="50" |Process B duration | ||
|- | |- | ||
| 2 | | 2 | ||
| Line 124: | Line 128: | ||
| Travka 20 | | Travka 20 | ||
| 34 cycles or 6:14 mins | | 34 cycles or 6:14 mins | ||
|} | |||
|+ '''Wafers''' | |||
|- | |||
! width="50" |Wafer number | |||
! width="50" |Mask | |||
! width="50" |Process B duration | |||
|- | |- | ||
| 11 | | 11 | ||
| Line 148: | Line 158: | ||
| Travka 65 | | Travka 65 | ||
| 34 cycles or 6:14 mins | | 34 cycles or 6:14 mins | ||
|} | |||
| STYLE="vertical-align: top"| | |||
{| border = 1 | |||
{| | |||
| STYLE="vertical-align: top"| | |||
{| border = 1 | |||
|+ '''Travka 05: A-line 2 µm to 25 µm fields''' | |||
! width="50" |Trench width (µm) | |||
! width="50" |Ridge width (µm) | |||
! width="50" |Period width (µm) | |||
! width="50" |Total periods | |||
! width="50" |Width of array (µm) | |||
|- | |||
|2||38||40||2||80 | |||
|- | |||
|3||57||60||3||180 | |||
|- | |||
|4||76||80||2||160 | |||
|- | |||
|6||114||120||1||120 | |||
|- | |||
|8||152||160||1||160 | |||
|- | |||
|10||190||200||1||200 | |||
|- | |||
|15||285||300||1||300 | |||
|- | |||
|25||475||500||1||500 | |||
|} | |||
| STYLE="vertical-align: top"| | |||
{| border = 1 | |||
|+ '''Travka 05: A-line 40 µm to 300 µm fields''' | |||
|- | |||
! width="50" |Trench width (µm) | |||
! width="50" |Ridge width (µm) | |||
! width="50" |Period width (µm) | |||
! width="50" |Total periods | |||
! width="50" |Width of array (µm) | |||
|- | |||
|40||760||800||1||800 | |||
|- | |||
|50||950||1000||1||1000 | |||
|- | |||
|75||1425||1500||1||1500 | |||
|- | |||
|100||1900||2000||1||2000 | |||
|- | |||
|150||2850||3000||1||3000 | |||
|- | |||
|200||3800||4000||1||4000 | |||
|- | |||
|300||5700||6000||1||6000 | |||
|} | |||
|} | |} | ||
Revision as of 15:22, 23 January 2013
Process B
Process B is labelled Via (30μm diameter) 100μm depth. In the acceptance test the process was run on a 150 mm SPTS wafer with 12-13 % etch load.
| Parameter | Specification | Average result |
|---|---|---|
| Etch rate (µm/min) | > 10 | 10.7 |
| Etched depth (µm) | 100 | 107 |
| Scallop size (nm) | < 800 | 685 |
| Profile (degs) | 91 +/- 1 | 90.7 |
| Selectivity to AZ photoresist | > 100 | 183 |
| Undercut (µm) | <1.5 | 0.89 |
| Uniformity (%) | < 3.5 | 2.7 |
| Repeatability (%) | <4 | 0.47 |
| Main etch (D->E) | Etch | Dep |
|---|---|---|
| Gas flow (sccm) | SF6 350 O2 35 | C4F8 200 |
| Cycle time (secs) | 7.0 | 4.0 |
| Pressure (mtorr) | 20 (1.5 s) 100 | 25 |
| Coil power (W) | 2800 | 2000 |
| Platen power (W) | 130 (1.5) 40 | 0 |
| Cycles | 55 (process time 10:05) | |
| Common | Temperature 10 degs, HBC 10 torr, Short funnel, with baffle & 5mm spacers | |
Experiment with process B performance
Purpose
Perhaps the most commonly occuring question posed by users of the dry etch tools is something like ' I want to etch my trenches down to a depth of 40 microns, how long should I etch?'. The answer is that it depends on the width of the trench and on the etch load of your design (that is how many percent of the wafer it etched).
An experiment has been set up to investigate the etched depth of a number of different trenches (with widths ranging from 2 microns to 300 microns) as a function of etch load (the exposed area ranges from 5 % to 65 %)
Results
A number of wafers are patterned with the travka masks in 4 microns of AZ photoresist. The wafers are then etc
|
|||||||||||||||||||||
| Wafer number | Mask | Process B duration | |||||||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| 11 | Travka 35 | 17 cycles or 3:07 mins | |||||||||||||||||||
| 12 | Travka 35 | 34 cycles or 6:14 mins | |||||||||||||||||||
| 14 | Travka 50 | 17 cycles or 3:07 mins | |||||||||||||||||||
| 15 | Travka 50 | 34 cycles or 6:14 mins | |||||||||||||||||||
| 17 | Travka 65 | 17 cycles or 3:07 mins | |||||||||||||||||||
| 18 | Travka 65 | 34 cycles or 6:14 mins |
| STYLE="vertical-align: top"|
|
|
- The results of process B after 17 and 34 cycles of etching
-
-
The 60 nm trenches