Latest revision as of 08:29, 25 June 2026
Plasma Asher 4 and 5
Product name: PVA Tepla Gigabatch 380M
Year of purchase: 2024
Descum of AZ 5214E on 100 mm wafers. The descum process development was done for a single substrate, as well as 3 substrates (for decreased ashing rate and improved ashing uniformity). The substrates were placed vertically in the glass boat.
-
Single vertical substrate
-
3 vertical substrates:
Dummy - Test - Dummy
For the 3 substrates only the center substrate was used for testing, the front and back wafers were used as dummy wafers. The wafers were placed in consecutive slots - when running multiple wafers in this way, the first and last wafers should always be dummy wafers.
The user manual, risk assessment, and contact information can be found in LabManager - requires login
Typical descum parameters
Tested with 1.5 µm AZ 5214E on 100 mm silicon substrate.
- O2: 100 sccm
- N2: 100 sccm
- Pressure (DSC): 1.3 mbar
- Power: 200 W
- Chamber temperature at start (with door closed): 30°C
- Time (single wafer): 5-10 minutes = 35-72 nm ashed
- Time (multiple wafers): 10-15 minutes = 40-80 nm ashed
| Single substrate | Center of 3 substrates | |
|---|---|---|
| Test results: ashing rate | 5.7 ±2.1 nm/min | 3.8 ±1.6 nm/min |
| Test results: non-uniformity | 0.6 ±0.4% | 0.4 ±0.2% |
| Wafers | 1 | 3 |
| Wafer size | 100 mm | 100 mm |
| Boat position | Center of chamber | Center of chamber |
| Test wafer position | Center of boat | Center of boat |
| Total gas flow rate | 200 sccm | 200 sccm |
| Gas mix ratio | 50% N2 | 50% N2 |
| Chamber pressure | 1.3 mbar | 1.3 mbar |
| Power | 200 W | 200 W |
| Test processing time | Tested parameter | Tested parameter |
| Test average temperature | 33°C | 33°C |
Single wafer descum ashing rate and uniformity for plasma asher 4 & 5

| Ashing time [min]: | 1 | 2 | 5 | 10 | 15 |
|---|---|---|---|---|---|
| Ashing amount [nm]: | 5.2 | 6.2 | 35.1 | 72.3 | 87.1 |
| Ashing rate [nm/min]: | 5.2 | 3.1 | 7.0 | 7.2 | 5.8 |
| Ashing time [min]: | 1 | 2 | 5 | 10 | 15 |
|---|---|---|---|---|---|
| Pre-descum film thickness range [nm]: | 11 | 12 | 10 | 11 | 9 |
| Pre-descum non-uniformity [%]: | 0.37 | 0.40 | 0.33 | 0.37 | 0.30 |
| Post-descum film thickness range [nm]: | 10 | 10 | 12 | 19 | 33 |
| Post-descum non-uniformity [%]: | 0.33 | 0.33 | 0.41 | 0.66 | 1.18 |
Multi wafer descum ashing rate and uniformity for plasma asher 4 & 5

| Ashing time [min]: | 1 | 2 | 5 | 10 | 15 |
|---|---|---|---|---|---|
| Ashing amount [nm]: | 4.3 | 6.7 | 10.1 | 39.5 | 78.8 |
| Ashing rate [nm/min]: | 4.3 | 3.4 | 2.0 | 4.0 | 5.3 |
| Ashing time [min]: | 1 | 2 | 5 | 10 | 15 |
|---|---|---|---|---|---|
| Pre-descum film thickness range [nm]: | 11 | 13 | 11 | 12 | 14 |
| Pre-descum non-uniformity [%]: | 0.37 | 0.43 | 0.37 | 0.40 | 0.46 |
| Post-descum film thickness range [nm]: | 11 | 9 | 10 | 12 | 21 |
| Post-descum non-uniformity [%]: | 0.37 | 0.30 | 0.33 | 0.41 | 0.74 |
Comparison between single substrate processing and multi substrate processing for plasma asher 4 & 5
Processing a single substrate using the standard descum settings will provide users with a relatively controllable and uniform process. Adding dummy substrates in close proximity with the process substrate will reduce the ashing rate and improve the uniformity:
-
Ashing amount
-
Ashing rate
-
Non-uniformity
Comparison of ashing rate between substrate sizes