Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch: Difference between revisions

From LabAdviser
Jml (talk | contribs)
No edit summary
Jml (talk | contribs)
No edit summary
Line 147: Line 147:


*[[Specific Process Knowledge/Etch/ICP Metal Etcher|ICP Metal Etch nanoetch]]
*[[Specific Process Knowledge/Etch/ICP Metal Etcher|ICP Metal Etch nanoetch]]
*[[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142-pxnano2|nano1.42 versus pxnano2]]
*[[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142-pxnano2|Nanoetch contest: DRIE-Pegasus versus ASE (nano1.42 versus pxnano2)]]

Revision as of 09:06, 23 August 2011

Recipe nano1.0 nano1.1 nano1.2 nano1.3 nano1.21 nano1.4 nano1.41 nano1.42 nano1.43
C4F8 (sccm) 52 52 52 52 75 75 75 75 75
SF6 (sccm) 38 38 38 38 38 38 38 38 38
O2 (sccm) 0 0 0 0 0 0 0 0 0
Coil power (W) 800 (F) 600 (F) 800 (F) 600 (F) 800 (F) 800 (F) 800 (F) 800 (F) 800 (F)
Platen power (W) 50 50 50 40 50 50 75 40 30
Pressure (mtorr) 4 4 4 4 4 4 4 4 4
Temperature (degs C) 10 10 -10 -10 -10 -20 -20 -20 -20
Process time (s) 120 120 120 120 120 120 120 120 120
Etch rates (nm/min)
Averages 295 228 299 235 183 183 166 160 148
Std. Dev 36 29 37 20 9 9 9 8 6
Zep etch rate (nm/min)
172 95 94 69 67 101 65 55
Sidewall angle (degrees)
Averages 93 94 92 94 91 91 90 90 90
Std. Dev 1 1 0 1 0 0 1 0 0
CD loss (nm pr edge)
Averages -11 -13 -17 -10 -10 -10 -20 -13 -24
Std. Dev 12 10 11 14 15 15 16 15 21
Bowing (nm)
Averages 31 42 13 16 6 6 3 -3 0
Std. Dev 7 6 4 3 2 2 2 3 1
Bottom curvature
Averages -45 -45 -44 -43 -32 -32 -34 -32 -39
Std. Dev 5 7 4 9 10 10 9 8 9