Ething of CLuminium can be done either wet or dry. For wet etching please see below on this page. Dry etching can be done either with [[Specific Process Knowledge/Etch/ICP Metal Etcher|ICP]] using Chlorine chemistry or with [[Specific Process Knowledge/Etch/IBE/IBSD Ionfab 300|IBE]] by sputtering with Ar ions. | |||
==Wet Aluminium Etch== | ==Wet Aluminium Etch== | ||
[[Image:Wet_Al_etch.jpg|300x300px|thumb|Wet Aluminium Etch: Positioned in cleanroom 4]] | [[Image:Wet_Al_etch.jpg|300x300px|thumb|Wet Aluminium Etch: Positioned in cleanroom 4]] | ||
Revision as of 13:55, 18 July 2011
Ething of CLuminium can be done either wet or dry. For wet etching please see below on this page. Dry etching can be done either with ICP using Chlorine chemistry or with IBE by sputtering with Ar ions.
Wet Aluminium Etch

Wet etching of aluminium is done with two different solutions:
- HO:HPO 1:2 at 50 oC
- Pre-mixed etch solution: PES 77-19-04 at 20 oC
Both solutions are used in the Aluminium etch bath shown to the right. It must be written on which one is in. Solution no. 1 is the most used solution for etching aluminium. Solution no. 2 is primarily for etching aluminium mixed with a small percentage of silicon.
Comparing the two solutions
| Aluminium Etch 1 | Aluminium Etch 2 | |
|---|---|---|
| General description | Etch of pure aluminium | Etch of aluminium + 1.5% Si |
| Chemical solution | HO:HPO 1:2 | PES 77-19-04 |
| Process temperature | 50 oC | 20 oC |
| Possible masking materials | Photoresist (1.5 µm AZ5214E) | Photoresist (1.5 µm AZ5214E) |
| Etch rate | ~100 nm/min (Pure Al) | ~60 nm/min |
| Batch size | 1-25 wafers at a time | 1-25 wafer at a time |
| Size of substrate | 4" wafers | 4" wafers |
| Allowed materials |
|
|
Dry Aluminium Etch
Our ICP Metal Etch tool allows you to dry etch aluminium.