Resist info
- we used a 10 % HSQ resist for a dose test. The resist info sheet could be found her.
- spinning: in labspin 3000rpm for 40s with 2s ramp (1500 acceleration) then bake for 2 min at 165 C
- Exposure: At 12nA ap6 (spot size 10 nm) in JEOL 9500
- Dose test with structures (3x3)
- Develop for 90s using manual TMAH developer
- Optical and SEM images and analysis
Results
Below is overview optical images of the developed pattern:

SEM images were recorded and analyzed from the structure shown below:

The measured and designed critical dimension are plotted vs the doses below:

The line width roughness (LWR) is plotted vs CD below:

.