Jump to content

Specific Process Knowledge/Lithography/EBeamLithography/HSQ Dose Test: Difference between revisions

From LabAdviser
Rawta (talk | contribs)
No edit summary
Rawta (talk | contribs)
Line 13: Line 13:
[[File:Dose test optical.png|frameless|625x625px|dose test optical images|left]]
[[File:Dose test optical.png|frameless|625x625px|dose test optical images|left]]


SEM images were recorded and analyzed from the structure shown below:<gallery>
SEM images were recorded and analyzed from the structure shown below:
File:Design.png
[[File:design.png|frameless|625x625px|dose test optical images|left]]
</gallery>
 
The measured and designed critical dimension are plotted vs the doses below:<gallery>
The measured and designed critical dimension are plotted vs the doses below:
File:CD vs dose.png
[[File:CD vs dose.png|frameless|625x625px|dose test optical images|left]]
</gallery>
 
The line width roughness (LWR) is plotted vs CD below: <gallery>
The line width roughness (LWR) is plotted vs CD below:  
File:LWR vs CD.png
[[File:LWR vs CD.png|frameless|625x625px|dose test optical images|left]]
</gallery>
 
.
.

Revision as of 14:11, 9 September 2025

Resist info

  • we used a 10 % HSQ resist for a dose test. The resist info sheet could be found her.
  • spinning: in labspin 3000rpm for 40s with 2s ramp (1500 acceleration) then bake for 2 min at 165 C
  • Exposure: At 12nA ap6 (spot size 10 nm) in JEOL 9500
    • Dose test with structures (3x3)
    • Develop for 90s using manual TMAH developer
    • Optical and SEM images and analysis  

Results

Below is overview optical images of the developed pattern:

dose test optical images
dose test optical images

SEM images were recorded and analyzed from the structure shown below:

dose test optical images
dose test optical images

The measured and designed critical dimension are plotted vs the doses below:

dose test optical images
dose test optical images

The line width roughness (LWR) is plotted vs CD below:

dose test optical images